I haven't entered this thread up to now because Doug said it all, but I
disagree with the notion that contamination testing is unnecessary with
RMA fluxes, for several reasons.
1) How do you know what levels and types of contamination were present
on the bare board and components before soldering?
2) How do you know whether all the halides in the flux have been
deactivated?
3) How do you know whether the cleaning process has not removed the
rosin but left the activators?
4) How do you know that metal halides have been removed?
Brian
- bogert wrote:
> January 6, 2008
>
> If the solder flux used is RMA or equivalent, is there any real benefit
> to doing a cleanliness test? I have reviewed OEM cleanliness test
> resords at several OEMs and the data I reviewed shows folks rarely, if
> ever fail this test.
>
>
>> From: Graham Collins <[log in to unmask]>
>> Reply-To: TechNet E-Mail Forum <[log in to unmask]>,
>> [log in to unmask]
>> To: [log in to unmask]
>> Subject: Re: [TN] specifying board cleanliness
>> Date: Thu, 3 Jan 2008 11:09:58 -0400
>>
>> Happy New Year Phil!
>> Well, "it depends"...
>>
>> First question is how clean do you need them to be? Depends on the
>> application and environment. Second question is what sort of assembly
>> process the CM is using - if "no clean" then they will be justifiably
>> opposed to cleanliness testing.
>>
>> The generic callout that we most commonly see on drawings is "clean per
>> J-STD-001 C-22" - which translates into clean the assembly, both sides,
>> and then do an ionic contamination test with a upper limit of 1.56
>> micrograms / cm2 NaCl equivalent contamination. I'm not sure why
>> J-STD-001 gives an option to only clean one side - never seen that
>> process in use. Anyway, a starting point...
>>
>> regards,
>>
>> Graham Collins
>> Halifax Production Engineering
>> L-3 communications Electronic Systems
>> (902) 873-2000 ext. 6215
>>
>>
>> -----Original Message-----
>> From: TechNet [mailto:[log in to unmask]] On Behalf Of Phil Nutting
>> Sent: Thursday, January 03, 2008 10:45 AM
>> To: [log in to unmask]
>> Subject: [TN] specifying board cleanliness
>>
>> Good Morning and Happy New Year to All,
>>
>> Let me start by confessing my ignorance relative to cleanliness of
>> circuit boards. We have no idea what numbers to specify that fit into
>> the IPC testing methods for board cleanliness. If I tell my CMs to make
>> the boards clean, it would be good to specify a target value and or test
>> method.
>>
>> Can someone give me some guidance on how to chose these specifications?
>> What are worth while tests and which ones are window dressing?
>>
>> I've read through some of the IPC tests methods and my head hurts.
>>
>> Thanks in advance,
>>
>> Phil Nutting
>>
>> Note: All the information contained in this e-mail and its attachments
>> is proprietary to Kaiser Systems, Inc. and it may not be reproduced
>> without the prior written permission of sender. If you have received
>> this email in error, please immediately return it to sender and delete
>> the copy you received.
>>
>> ---------------------------------------------------
>> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
>> unsubscribe, send a message to [log in to unmask] with following text in
>> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
>> (re-start) delivery of Technet send e-mail to [log in to unmask]: SET
>> Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
>> posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
>> archives of previous posts at: http://listserv.ipc.org/archives Please
>> visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
>> additional information, or contact Keach Sasamori at [log in to unmask] or
>> 847-615-7100 ext.2815
>> -----------------------------------------------------
>>
>> ---------------------------------------------------
>> Technet Mail List provided as a service by IPC using LISTSERV 15.0
>> To unsubscribe, send a message to [log in to unmask] with following text in
>> the BODY (NOT the subject field): SIGNOFF Technet
>> To temporarily halt or (re-start) delivery of Technet send e-mail to
>> [log in to unmask]: SET Technet NOMAIL or (MAIL)
>> To receive ONE mailing per day of all the posts: send e-mail to
>> [log in to unmask]: SET Technet Digest
>> Search the archives of previous posts at:
>> http://listserv.ipc.org/archives
>> Please visit IPC web site
>> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
>> information, or contact Keach Sasamori at [log in to unmask] or
>> 847-615-7100 ext.2815
>> -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
> ext.2815
> -----------------------------------------------------
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|