TECHNET Archives

January 2008

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Igoshev, Vladimir" <[log in to unmask]>
Date:
Thu, 17 Jan 2008 09:33:14 -0600
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Content-Transfer-Encoding:
quoted-printable
Subject:
From:
"David D. Hillman" <[log in to unmask]>
X-cc:
In-Reply-To:
Content-Type:
text/plain; charset="ISO-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (275 lines)
Hi Vlad - I think Werner and I are on the same page - the solderability is 
going to be a function of the IMC surface being wettable during the 
soldering process. If wetting can't be achieved (due to any number of 
circumstances) then the solder joint integrity is degraded/damaged.

Dave



"Igoshev, Vladimir" <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
01/17/2008 09:25 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
"Igoshev, Vladimir" <[log in to unmask]>


To
[log in to unmask]
cc

Subject
Re: [TN] SV: [TN] SV: [TN] Solderability of Tin-Gold Intermetallic






Hi Dave,

I remember your original e-mail stating that it shouldn't be any 
solderabilty problemsa, but hen Wernber came up saying otherwise.

Therefore, I think the answer is still up in the air. That is why I tried 
to re-stated it in a slightly different way :-)


Regards,

Vladimir

----- Original Message -----
From: [log in to unmask] <[log in to unmask]>
To: Igoshev, Vladimir
Cc: TechNet E-Mail Forum <[log in to unmask]>
Sent: Thu Jan 17 10:05:55 2008
Subject: RE: [TN] SV: [TN] SV: [TN] Solderability of Tin-Gold 
Intermetallic


Hi Vlad! I thought we had answered the solderability questions. 
Intermetallic phases are typically as solderable as the parent metals 
until they become oxidized (then they are impossible to solder!). So as 
long as the Au/Sn IMC phases are not oxidized as a function of Bev's 
soldering process, there should be not issue. Both Inge's and my photos 
that Steve posted show that a non-oxidized Au/Sn IMC is fully integrated 
into the solder joint structure and I don't believe Bev's situation is any 
different. The gold embrittlement discussion that has streamed along is 
just the TechNet metallurgists having way too much fun. 

Dave 



"Igoshev, Vladimir" <[log in to unmask]> 

01/17/2008 08:56 AM 
To
                 "TechNet E-Mail Forum" <[log in to unmask]>, 
[log in to unmask] 
cc
 
Subject
                 RE: [TN] SV: [TN] SV: [TN] Solderability of Tin-Gold 
Intermetallic

 




Dave and almost everyone else,

I believe we are missing the point. Bev has NEVER asked whether "his" 
joints can experience gold embrittlement, but whether the presence of 
gold/tin intermetallics can/will affect the solderability.

I think he is not the only one who would want to know the answer and so 
far the answer is almost unknown.

As far as I remember, Werner said that the solderability to AuSn4 is poor. 
Are their any papers with data? 

I think it would be great to have data on solderability of of common 
solders (Pb-free and PB-Sn) to Sn-Au alloys (with Au content from 30% down 
to 0).


Regards,

Vladimir 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: Thursday, January 17, 2008 8:21 AM
To: [log in to unmask]
Subject: Re: [TN] SV: [TN] SV: [TN] Solderability of Tin-Gold 
Intermetallic

Hi Bev - Arguably, the "magic" industry number is "3%"  for gold content. 
The AuSn4 phase formation kicks into gear around that percentage. The 
amount of gold you have is low and provided it is well distributed through 

out the solder joint (e.g. not segregated in one area) then you should not 

have any solder joint integrity issues. Some of the work done by Bester (
M. Bester, ?Metallurgical Aspects of Soldering Gold and Gold Plating?, 
InterNEPCON Proceedings, 1968) shows that 1-2% gold actually strengthens 
the solder joint a bit. I believe you have a low-to-no risk situation.

Dave



"Bev Christian" <[log in to unmask]> 
01/16/2008 04:24 PM

To
"TechNet E-Mail Forum" <[log in to unmask]>, <[log in to unmask]>
cc

Subject
RE: [TN] SV: [TN] SV: [TN] Solderability of Tin-Gold Intermetallic






Dave,
I only have 0.8 to 1.2% gold in the solder balls - as determined by XRF.
Bev

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: Wednesday, January 16, 2008 5:06 PM
To: [log in to unmask]
Subject: Re: [TN] SV: [TN] SV: [TN] Solderability of Tin-Gold 
Intermetallic

Hi gang! Steve - I just sent you another set of photos showing a solder 
joint that has gold embrittlement. Bev - if you have a solder joint that 
contains the AuSn4 microstructure phase then you have an indication that 
your overall composition has exceeded the "magical" 4% limit.  The 
presence of the AuSn4 platelets cause the solder joint to behave in a 
brittle manner when subjected to some use environments. The formation of 
the AuSn4 phase isn't going to interfere with the formation of your solder 


joint but they do result in solder joint integrity degradation. The 
pretinning of gold plated component leads is an attempt to replace the 
gold with a solder coating and lower the overall total percentage of gold 
that would exist in the solder joint - the lower the overall solder joint 
gold content, the lower the likelihood for the AuSn4 phase to form.

Dave Hillman
Rockwell Collins
[log in to unmask]




Steve Gregory <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
01/16/2008 03:35 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Steve Gregory <[log in to unmask]>


To
[log in to unmask]
cc

Subject
Re: [TN] SV: [TN] SV: [TN] Solderability of Tin-Gold Intermetallic






Hi Inge ol' pal!

I went back and looked on my pages, and am not sure if they're still 
there. But one of these might be:

http://stevezeva.homestead.com/files/fracture_bad.jpg

http://stevezeva.homestead.com/files/fracture_bad_2.jpg


Steve




-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Hfjord
Sent: Wednesday, January 16, 2008 3:09 PM
To: [log in to unmask]
Subject: [TN] SV: [TN] SV: [TN] Solderability of Tin-Gold Intermetallic

Not really true, the Scottish blood in my veines tells me to be careful 
with money, the kyrgise blood makes me crush the table, therefore, noone 
can actually be under it. 

I think there are pictures from my large AuSn platelets somewhere on 
Gregory's wall. If not, I can probably dig them up again from some old 
report. If such crystals are abundant in a solder joint, the components 
may just jump off the board when giving a mechanical shock.

/Inge

-----Ursprungligt meddelande-----
Från: TechNet [mailto:[log in to unmask]] För Werner Engelmaier /*
Skickat: den 16 januari 2008 20:30
Till: [log in to unmask]
Ämne: Re: [TN] SV: [TN] Solderability of Tin-Gold Intermetallic

Hi Inge,
As usual people are well advised not to argue with a (this) Swede; 1) he 
usually knows what he is talking about, and 2) if not, he will drink you 
under the table.
The IMCs formed by Sn/Pb, and Sn/Ag as well, are platellet-shaped crystals 


(in cross-section they may look like needles but are always plateletts), 
and I have seen no evidence that they are solderable. Solderability simply 


depends on how much Sn, or SnPb, to which you wet, is present. So the 
amount of these IMCs affect both solderability as well as 
Au/Ag-embrittlement.
Inge, how is Gerd? I sure have not heard anything about him for some time.



Werner















---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2