It's a misunderstanding, that intermetallics like AuSn or its sisters have
bad wetting. In fact, the surface energy of such intermetallics is perfectly
matching Tin or Tin/Lead solder and the wetting is good. It's the
crystallographic structure, that decides whether there will be a
sufficiently strong joint or not. If large crystals or needles or disks are
formed, mechanical forces have a tendency to concentrate along these
features, thus resulting in a weak and brittle joint. One of my friends, dr
Becker, made a pioneer job in the 60s, calculating the famous 4% Au level,
which one has caused little of gold content paranoia. In his paper, he
points out, that it's not the 4%Au in itself, that is dangerous, but the
said macro crystal forming. I have presented such macro crystals, Werner
have the photos.
Inge
-----Ursprungligt meddelande-----
Från: TechNet [mailto:[log in to unmask]] För Bev Christian
Skickat: den 16 januari 2008 15:39
Till: [log in to unmask]
Ämne: Re: [TN] Solderability of Tin-Gold Intermetallic
Bingo! This is the type of answer I was looking for. Thx.
Bev
RIM
----- Original Message -----
From: Wenger, George M. <[log in to unmask]>
To: Bev Christian; TechNet E-Mail Forum <[log in to unmask]>
Sent: Wed Jan 16 09:20:00 2008
Subject: RE: [TN] Solderability of Tin-Gold Intermetallic
Bev,
I'm not sure I can give you a direct answer for tin but I can give you
an answer for SnPb solder. In the RF world there are lots of gold
plated components that can have very thick gold (>2.5um). Because of
solder joint reliability reliability concerns it has been standard
practice to pre-tin (expose to SnPb wave or use a double dip in to
solder pots) to dissolve most of the gold) and the resulting pre-tinned
surface does contain some gold. The amount of gold remaining in the
solder on the surface of the components is dependent on the quality of
the pr-tinning process. However, we've seen many surfaces of pre-tinned
components with up to at least 4% gold and have not seen any
solderability issues.
Regards,
George
George M. Wenger
Senior Principle FMA / Reliability Engineer
CommScope / Andrew Wireless Solutions
40 Technology Drive, Warren, NJ 07059 (908) 546-4531
[log in to unmask]
-----Original Message-----
From: Bev Christian [mailto:[log in to unmask]]
Sent: Wednesday, January 16, 2008 9:04 AM
To: Wenger, George M.; TechNet E-Mail Forum
Subject: RE: [TN] Solderability of Tin-Gold Intermetallic
George,
Correct of course. That is what I meant. How about my question?
Bev
RIM
-----Original Message-----
From: Wenger, George M. [mailto:[log in to unmask]]
Sent: Wednesday, January 16, 2008 9:03 AM
To: TechNet E-Mail Forum; Bev Christian
Subject: RE: [TN] Solderability of Tin-Gold Intermetallic
Bev,
I think I would re-state your first sentence. "We all know that
tin-copper intermetallic that has come to the surface and been exposed
to the environment has terrible solderability." I view tin-copper as
the glue layer between solder and copper when solder touches copper and
forms an intermetallic the solder above the intermetallic must wet it
otherwise it would fall off.
Regards,
George
George M. Wenger
Senior Principle FMA / Reliability Engineer CommScope / Andrew Wireless
Solutions 40 Technology Drive, Warren, NJ 07059 (908) 546-4531
[log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Bev Christian
Sent: Wednesday, January 16, 2008 8:52 AM
To: [log in to unmask]
Subject: [TN] Solderability of Tin-Gold Intermetallic
Technetters,
We all know that the tin-copper intermetallic has terrible
solderability. I also know there are high melting tin-gold solders. My
question is: what is the solderability of surfaces of tin with small
amounts of gold (<4%) in it? As good as 100% tin, better, worse? If
worse, how much so?
Bev
RIM
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential
information, privileged material (including material protected by the
solicitor-client or other applicable privileges), or constitute
non-public information. Any use of this information by anyone other than
the intended recipient is prohibited. If you have received this
transmission in error, please immediately reply to the sender and delete
this information from your system. Use, dissemination, distribution, or
reproduction of this transmission by unintended recipients is not
authorized and may be unlawful.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
------------------------------------------------------------------------
------------------------
This message is for the designated recipient only and may contain
privileged, proprietary, or otherwise private information.
If you have received it in error, please notify the sender immediately
and delete the original. Any unauthorized use of this email is
prohibited.
------------------------------------------------------------------------
------------------------
[mf2]
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential
information, privileged material (including material protected by the
solicitor-client or other applicable privileges), or constitute
non-public information. Any use of this information by anyone other than
the intended recipient is prohibited. If you have received this
transmission in error, please immediately reply to the sender and delete
this information from your system. Use, dissemination, distribution, or
reproduction of this transmission by unintended recipients is not
authorized and may be unlawful.
----------------------------------------------------------------------------
--------------------
This message is for the designated recipient only and may
contain privileged, proprietary, or otherwise private information.
If you have received it in error, please notify the sender
immediately and delete the original. Any unauthorized use of
this email is prohibited.
----------------------------------------------------------------------------
--------------------
[mf2]
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential
information, privileged material (including material protected by the
solicitor-client or other applicable privileges), or constitute non-public
information. Any use of this information by anyone other than the intended
recipient is prohibited. If you have received this transmission in error,
please immediately reply to the sender and delete this information from your
system. Use, dissemination, distribution, or reproduction of this
transmission by unintended recipients is not authorized and may be unlawful.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|