Hi Dave! The idea that a faster cooling rate results in improved solder
joint integrity is an tribal myth. A faster cooling rate does result in a
finer initial solder joint microstructure but after 48 hours that finer
grain microstructure undergoes recystalization to a larger grain structure
negating any possible solder joint integrity improvements that might have
been achieved.
Dave Hillman
Rockwell Collins
[log in to unmask]
David Tremmel <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
12/05/2007 09:34 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
David Tremmel <[log in to unmask]>
To
[log in to unmask]
cc
Subject
Re: [TN] Reflow Oven Cooling Zone Question
Hello,
The acceptability of the last zone operating at 160°C-170°C may be one of
the cooling rate of the assembly.
A faster cooling rate (4°C per second is usually recommended) creates a
finer grain structure in the solder which creates a more reliable solder
joint.
If the last zone of the oven is only giving you a cooling rate of less
than
3°, then you may be creating reliability issues for your self in the shop
or
in the form or field returns.
I am not a guru so that is only my .2 cents.
Thank you,
David Tremmel
http://ValuRecovery.com
VALUE RECOVERY
Quality is the nature of the service
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leland Woodall
Sent: Miércoles, 05 de Diciembre de 2007 09:18 a.m.
To: [log in to unmask]
Subject: [TN] Reflow Oven Cooling Zone Question
Good morning, everyone!
Lately we've had a slight issue with one of our reflow ovens. We have
set our temp parameter for the last zone at 150 degrees C. When we
first received this oven we had no problem with maintaining this zone as
prescribed.
I assume we have an insulation barrier that's breaking down and causing
this situation.
Anyway, how critical is this cooling zone? If the oven is no longer
able to maintain the current setpoint, would it harm anything for this
zone to move up in the 160 to 170 degree range?
We're running a pb-free process here, just in case it makes any
difference...
Thanks in advance for your help.
Leland Woodall
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|