TECHNET Archives

October 2007

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Thu, 11 Oct 2007 09:50:39 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Creswick, Steven" <[log in to unmask]>
Subject:
From:
"Creswick, Steven" <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="iso-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (109 lines)
Victor,

From a practical point of view, that would be quite difficult.  The actual internal gas volume of these devices is very, very small.

I'm not sure I would believe any number I got.

As a next level up, one could do a dye penetrant test.

Steve

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Victor G. Hernandez
Sent: Thursday, October 11, 2007 9:45 AM
To: [log in to unmask]
Subject: Re: [TN] Cracks in the body of glass diodes (JANTX1N4148UR1)

Did you conduct a hermetic Test?


Victor,

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: Thursday, October 11, 2007 7:38 AM
To: [log in to unmask]
Subject: Re: [TN] Cracks in the body of glass diodes (JANTX1N4148UR1)

Good Morning Juan!

I have your pictures posted. They are here:

http://stevezeva.homestead.com/files/JTX1N4148_UR1_003.jpg

http://stevezeva.homestead.com/files/JANTX1N4148_UR1_004.jpg

http://stevezeva.homestead.com/files/JANTX1N4148_UR1_001.jpg

I'm with Inge on this one. These cracks are in the body, not good. There is something I have noticed in two of the pictures, UR1_004 and UR_001, is that the glass seems discolored right next to the termination, which to me indicates that they may have been thermally shocked.

Do you know where these diodes were purchased from? Brokers maybe? Maybe salvaged off some boards? Poorly pre-tinned to restore solderability?

I wouldn't use them...

Steve Gregory



-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Juan T. Marugán
Sent: Thursday, October 11, 2007 5:25 AM
To: [log in to unmask]
Subject: [TN] Cracks in the body of glass diodes (JANTX1N4148UR1)

Good Morning,

In a certain number of SMD diodes we have detected what we consider as a crack in the glass body of the diode. This condition was already present in the diodes packaged in a reel, that is, before mounting in the PWAs.

What we cannot determine yet is if this condition could be acceptable. Could you help us through your valuable opinions?

PD: I have sent 3 photographs to Steve Gregory.

Thank you in advance. 

Juan T. Marugán López
Indra Sistemas SA
Supply Chain Management (SCM)
Production Quality
 
C/ Joaquín Rodrigo 11
28300 Aranjuez - Madrid (SPAIN)
 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

THE INFORMATION CONTAINED IN THIS E-MAIL MESSAGE AND ANY ATTACHMENTS SENT FROM GENTEX CORPORATION IS GENTEX CONFIDENTIAL INFORMATION INTENDED ONLY FOR THE PERSONAL USE OF THE INDIVIDUAL OR ENTITY NAMED ABOVE. If you are not the intended recipient, you are hereby notified that any review, distribution, or copying of this communication is strictly prohibited.  If you have received this communication in error, please immediately notify the sender by return e-mail, and delete this e-mail message and any attachments from your computer.  




---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest