Periodically I still see the F problem with bond pads, but it is increasingly rare.
Best regards,
Leo
Leo M. Higgins III, Ph.D.
Sr. Vice President, Engg and Technology
ASAT, Inc.
13809 Research Blvd., Suite 635
Austin, Texas 78750
office phone 512-249-4758
mobile 512-423-2002
[log in to unmask]
www.asat.com
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Hfjord
Sent: Thursday, September 06, 2007 2:52 PM
To: [log in to unmask]
Subject: [TN] SV: [TN] Semi guys, need support
Dear Vlad,
First image is 0.5 kV, next 2.0 kV, then 5 kV and finally 20 kV.
The numerous small grains and the pores are not normal for semi
metallization. The spectra is collected from areas with these protrusions
or grains. Compared with normal chips, no F present. The spectrometer has no
False F peaks. The only such peak is a very small Si peak, which is common
For many EDAX's. There IS Fluorine!
I got a message from Leo Higgins, his comment tells me he knows about semi
processes, which I do myself. I've done analysis for TI, MOTA, NG, XILINX
and some more, and I've seen a lot, especially from MESFETs and HBTs, but
these chips are little of a mystery because of the extremely bad wire
bondability. The problem is of course not to find in the epitaxial
processes, but in the metallisation chain. The fluorine problems used to be
found in the early time of semiconductors, and was well known, but I have
not seen that failure category for years and years. Maybe something happen
when this US company moved production to...erh..other countries.
Contaminated rinse water or contaminated vacuum/sputter equipments may also
be a source (very unusual with serious manufacturers).
Auger, yep, we have the machine not far away. FIB or TOFSIMS may also be of
interest.
The production of laser equipments is stopped because of these dirty little
creeps. They hoped I would give them good news, but I can't accept the
quality of these chips. If they ask for reference, I'll say a lion told me.
Inge
-----Ursprungligt meddelande-----
Från: TechNet [mailto:[log in to unmask]] För Igoshev, Vladimir
Skickat: den 6 september 2007 18:57
Till: [log in to unmask]
Ämne: Re: [TN] Semi guys, need support
Inge,
I don't see any 1kV images and don't quite understand what you mean by
referring to a "strange superficial structure".
Another point is the presence of F. The fact that the software shows it
DOES NOT mean it's there (and the actual spectrum you provided doesn't
tell it's there).
Regards,
Vladimir
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Hernefjord Ingemar
Sent: Thursday, September 06, 2007 10:01 AM
To: [log in to unmask]
Subject: [TN] Semi guys, need support
25 micron gold ball bonding bad yield, ball lifts, poor adhesion on Al
pads. Triple diff line tranceiver chip. Weird micrographic exteriour,
EDAX gives C,F,O, Cl,Cu,Al,Fe. Cu can be ppm alloy but the others
unwanted on semi chip bond pads I think. 1kV SEI SEM reveals strange
superficial structure. Chip not contaminated by us, fresh opened chip
trays show this face. Question: what semi manufacturing problem can this
be? Will post a few pics to Steve's gallery.
TrikeMan?
/Inge
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|