Dale and John,
This particular PCB is also from China, and the overall dimensions are
187 MM by 117 MM by 1.7 MM thick. It's a 6 layer board.
The only change the vendor has undergone (of which they've made us
aware) in the processing was an increase in their reflow screening temp.
It was increased from 243 C to 258 C, and it was done to help them
detect thin plating conditions in the vias.
This product has been lead-free since its inception...
Leland
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Dale Ritzen
Sent: Thursday, July 12, 2007 12:45 PM
To: [log in to unmask]
Subject: Re: [TN] PCB Fab Question Regarding Bow and Twist
John et al,
We, too, have started getting (within the last 6 months) raw PCBs with
pretty severe bow & twist problems directly from Chinese PCB shops. I
suppose they could be adding melamine to the fiberglass material, too...
Seriously, this has become a bad problem over the last 6 months. We have
even thought about dropping some of our Chinese board suppliers, but are
trying to exhaust all our "other" options (like looking under ALL the
rocks
here first) before we go draconian on them. Might just be in their haste
to
get product to their customers that they are hurrying the cooling stages
of
fabrication a bit, causing the material to contract more than it should.
Speculation at this point...
Dale Ritzen
Quality Manager
Austin Manufacturing Services
-----Original Message-----
From: John Burke [mailto:[log in to unmask]]
Sent: Thursday, July 12, 2007 11:20 AM
To: [log in to unmask]
Subject: Re: [TN] PCB Fab Question Regarding Bow and Twist
Leland, you have to relate the warpage on those boards to the distance
over
which you are measuring in the XY plane.
Did you switch to lead free in that time frame?
John
John Burke
(408) 515 4992
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leland Woodall
Sent: Thursday, July 12, 2007 9:03 AM
To: [log in to unmask]
Subject: [TN] PCB Fab Question Regarding Bow and Twist
Everyone,
I have a product that ran for almost a year with little or no problem.
Recently we've started seeing unsoldered pins on a 256 pin QFP, and
found the cause to be excessive twist in the board.
We have verified that no changes have been made to our process. Reflow
temps, cooling rates, conveyor speeds, rail parallelism, and transfers
are all good. We've checked incoming raw material and found only slight
deflection in a few specimens.
A couple of examples:
Incoming: 0.13 MM
B reflow: 0.66 MM
A reflow 1.98 MM
We've identified assemblies that have excessive twist after each of the
reflow operations, and our once good product is becoming an expensive
stepchild. We cannot mount twisted boards into cases because of too
much strain, and are forced to scrap this material.
What in the PCB manufacturing process might have changed that would
cause this scenario?
Thanks in advance for your input.
Leland
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|