re: 4 suggestions mentioned earlier
<Phil Bavaro is the master of the universe in this area>
1) via tenting top side only
As I understand your description this in not what you want to do. This may
be a planarity problem, no? Although you don't have to worry about the vias
venting into your solder joint.
2) via tenting bottom side only
Bad idea. Been there, done that. Take it to the bank, this will give you
solder voids. Via won't be completely filled by s/m but will block the
entrapped gasses from venting to backside.
3) via plugging from the bottom side
Full plugging is as a nearly an ideal condition as you can hope for. We do
a lot of this with great success. Not all fabs have the recipe yet.
If anything, preferred filling is from topside (with post planarization).
From either side OK as long as it's filled to top surface and planar at
the top (solder) surface to minimize venting/voiding problems into the
solder joint
4) via encroached
If by "via encroached" you mean encroaching on the via with soldermask on
the backside;
Then, yes we've done this a lot. This is arguably "the elegant" solution.
It allows solder venting through the via, thus minimizing voiding.
If pwb supplier uses s/m "tent breaker" approach(s/m aperture = drill minus
a few mil) then usually the via wets partially but solder never comes to
back sider surface.
If pwb supplier uses a "cheater via" approach (s/m aperture = drill plus a
few mil) then the via may substantially fill w/ solder but not come to the
surface. There isn't enough annular ring on the back side to allow solder
to wet and hold on a miniscus on the surface ring. Surface tension holds
the solder back into the via.]
5) None of the above:
If thru via drill is small (on order of 10 mils) resulting in an even
smaller finished via then just leave via open. It'll vent and not wet
through to other side.
Phil and I did a lot of this with great success. Not always the politically
expedient thing to do. Someone will push back in review cycle, not
understanding how it works or believing our empirical evidence of success.
In those cases we'd use method 3 or 4 (above) as a concession to their "If
there are any problems then the blood will be on your hands" threats.
At 09:17 AM 7/30/2007, Hogg, Blair K. wrote:
>If the via is in a pad, or a heatsink area under a device which is not
>normally covered with soldermask, would you put soldermask over just the
>via?
>
>-----Original Message-----
>From: TechNet [mailto:[log in to unmask]] On Behalf Of Whittaker, Dewey
>(EHCOE)
>Sent: Monday, July 30, 2007 10:28 AM
>To: [log in to unmask]
>Subject: Re: [TN] Via tenting
>
>I'll spare you the tribal knowledge of dual dwellings, but if long term
>reliability is a requirement choose one of the following:
>
>* A plated-over filled via using Taiyo or Peter's material(
>CB100 need not apply)
>
>* A tented via where both sides are capped and covered with a
>SMOBC per IPC-SM-840
>
>
>
>Dewey
>
>
>
>-----Original Message-----
>
>From: TechNet [mailto:[log in to unmask]] On Behalf Of West, Jim
>
>Sent: Friday, July 27, 2007 12:52 PM
>
>To: [log in to unmask]
>
>Subject: [TN] Via tenting
>
>
>
>Hi,
>
>
>
>We have an application where we are using a QFN/SON package that has one
>
>large exposed pad at the bottom of the package. In order to ensure good
>
>electrical characteristics and thermal protection, the chip manufacturer
>
>recommends a thermal pad via design. The recommendation is to use 6
>
>via's within the large pad placed on a 1.0mm pitch to help facilitate
>
>the thermal relief. In addition, they suggest 0.3mm diameter drill
>
>holes. There are several suggestions on what one would do to these
>
>via's to reduce the exposure of excess voiding during the reflow
>
>process. One suggestion is via tenting top side only, second suggestion
>
>is via tenting bottom side only, third suggestion is via plugging from
>
>the bottom side, and finally the fourth suggestion is via encroached
>
>from the bottom.
>
>
>
>As I look at these suggestions, I would probably utilize the via
>
>tenting top side only, since this would probably result in smaller
>
>voids, but one of the risks is a hindrance of proper paste printing.
>
>Options 2 and 3, I would think that there would be an increased in out
>
>gassing and voiding. The fourth option would cause reduced voiding, but
>
>could cause a lower standoff of the package, causing improper soldering
>
>conditions.
>
>
>
>
>
>Anyone have a thoughts/experience on how to handle this type of
>
>application?
>
>
>
>Best Regards,
>
>
>
>
>
>
>
>Jim West
>
>Engineering Manager
>
>Nexergy Inc.
>
>www.nexergy.com
>
>tel: (614) 351-6216
>
>fax: (614) 324-1979
>
>
>
>
>
>
>
>This email message and all attachments transmitted with it are intended
>solely for the use of the addressee(s) and may contain legally
>privileged, protected or confidential information. If you believe that
>you have received this message in error, please notify the sender
>immediately by email reply and please delete this message from your
>computer and destroy any copies.
>
>
>
>--------------------------------------------------------
>
>
>
>---------------------------------------------------
>
>Technet Mail List provided as a service by IPC using LISTSERV 15.0
>
>To unsubscribe, send a message to [log in to unmask] with following text
>in
>
>the BODY (NOT the subject field): SIGNOFF Technet
>
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>
>Search the archives of previous posts at:
>http://listserv.ipc.org/archives
>
>Please visit IPC web site
>http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
>information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
>ext.2815
>
>-----------------------------------------------------
>
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
>unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
>(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
>Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
>posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
>archives of previous posts at: http://listserv.ipc.org/archives Please
>visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
>additional information, or contact Keach Sasamori at [log in to unmask] or
>847-615-7100 ext.2815
>-----------------------------------------------------
>
>*******************************************************************
>This email and any files transmitted with it are confidential and
>intended solely for the use of the individual or entity to whom they
>are addressed. If you have received this email in error please notify
>the system manager.
>
>This footnote also confirms that this email message has been swept
>for the presence of computer viruses.
>
>www.Hubbell.com - Hubbell Incorporated
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>for additional information, or contact Keach Sasamori at [log in to unmask] or
>847-615-7100 ext.2815
>-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|