Even if you do all the thing that everyone says, you could still have
difficulties.
Immersion tin seems to be a very supplier dependent process so that the
possibility of batch to batch variation, differences in supplier performance
for the same specification etc, is higher than other finishes. Shelf
life/storage certainly does need to be controlled, and can be much shorter
than thought.
If you view the first side reflow as an artificial ageing process you can
see that you easily can slip in to difficulty even with a batch of boards
that was previously OK on both sides.
Regards
Mike
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leo Higgins
Sent: Wednesday, July 18, 2007 10:46 AM
To: [log in to unmask]
Subject: Re: [TN] Immersion Tin
Hi folks,
In the different world of IC assy and pkgg, use of imm Sn on BGA pads
is not uncommon. After eutectic Sn-Pb flip chip reflow in Nitrogen with low
Oxygen (about 20ppm ), followed by several thermal processes at between 125
- 165C for substrate baking and underfill curing in air, PbFree SAC305 ball
attach is performed with excellent results. Imm Sn is about 1 um thick.
Thanks.
Best regards,
Leo
Leo M. Higgins III, Ph.D.
Sr. Vice President, Engg and Technology
ASAT, Inc.
13809 Research Blvd., Suite 635
Austin, Texas 78750
office phone 512-249-4758
mobile 512-423-2002
[log in to unmask]
www.asat.com
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Stadem, Richard D.
Sent: Tuesday, July 17, 2007 3:45 PM
To: [log in to unmask]
Subject: Re: [TN] Immersion Tin
Larry, Reuven
Any thickness of tin is going to oxidize somewhat after going through
two reflow passes. Even lead-free components that are baked out
overnight at 150 C show a marked darkening on the tin-plated
terminations, even with 90 uinches of tin or more. Circuit boards with
immersion tin finish are also susceptible to oxidation.
The nitrogen exposure is only in the reflow portion of the tunnel. But
it helps a little, as that is the hottest.
However, any time you heat tin above 100 deg. C or so, it oxidizes
somewhat quickly. That is one of the reasons (just one) that immersion
tin is not always a preferred finish. Is there a particular reason why
you wanted to use it?
You may wish to try immersion silver instead, but without looking at
your assembly configuration and its intended use it is hard to recommend
a finish.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Reuven Rokah
Sent: Tuesday, July 17, 2007 3:14 PM
To: [log in to unmask]
Subject: Re: [TN] Immersion Tin
The thickness of the Tin finish is below the minimum.
Short term solution:
Lower peak profile as possible.
Use Nitrogen
Long term
Replace supplier of PCBs
Corrective actions of existing supplier
Best Regards
Reuven ROKAH
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Larry K
Sent: Tuesday, July 17, 2007 10:35 PM
To: [log in to unmask]
Subject: [TN] Immersion Tin
We are having problems with solderability of the PCB on oursecond side
reflow. Everything looks good after reflowon the first side but when we
run the second side we have non-wetting of the pads of this side.
Just to ensure we were doing everything correctly,we switched sides
(we did the second side first and then did the first side as a second
reflow) and the problem was still after the second reflow. We are
thinking this validated our process because the side causing us problems
switched with our experiment. As I said in the suject line, this is
Immersion Tin. Any suggestions for a cure?
thanks,
Larry
---------------------------------
Get your own web address.
Have a HUGE year through Yahoo! Small Business.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
***This email, its content and any files transmitted with it are intended solely for the addressee(s) and may be legally privileged and/or confidential. If you are not the intended recipient please delete and contact the sender by return and delete the material from any computer. Any review, retransmission, dissemination or other use of, or taking of any action in reliance upon, this information by persons or entities other than the intended recipient is prohibited.
Messages sent via this medium may be subject to delays, non-delivery and unauthorized alteration. This email has been prepared using information believed by the author to be reliable and accurate, but Indium Corporation makes no warranty as to accuracy or completeness. In particular, Indium Corporation does not accept responsibility for changes made to this email after it was sent. Any opinions or recommendations expressed herein are solely those of the author. They may be subject to change without notice.***
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|