Hello,
Hope this helps.
1. We have determined dull joints are due to excessive washing. The
joints were always shiny after process and turned dull if parts were left
in water for too long. We eliminated residues and heat drying as
causes and were able to duplicate the dull appearance by exposing to
water for longer periods.
2. Alpha Metals has published a paper on white residues
http://www.alphametals.com/techsupport/tools/WhiteResiduesWaterSolu
bleFluxes121900.pdf
Regards,
Prashant
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------