TECHNET Archives

June 2007

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Jim Ma <[log in to unmask]>
Date:
Thu, 14 Jun 2007 07:58:26 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Stadem, Richard D." <[log in to unmask]>
Subject:
From:
"Stadem, Richard D." <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="us-ascii"
MIME-Version:
1.0
Parts/Attachments:
text/plain (69 lines)
If the surface finish is in fact ENIG (real ENIG as specified in per the
IPC standard) then the storage conditions should not cause any loss of
solderability. However, I still recommend all circuit boards be
dry-packed as if they were an MSD, because they are. Moisture saturation
in PWBs prior to reflow will lead to other issues not related to
solderability.

But real ENIG with a gold coverage of 2-5 uinches will not readily
oxidize or lose solderability, at least not within a year in an
environment free of harsh chemicals, especially chlorides.
I suspect that the boards that are the subject of this discussion were
not properly plated, and that the resulting level of phosphorus between
the gold and the nickel is higher than it should be, if they are in fact
ENIG. This does lead to a nickel oxide barrier forming over the nickel
underneath the gold. It is not always "Black Pad" per se, but a barrier
to soldering nonetheless.
This barrier can continue to grow long after the boards have been
soldered, and its growth is accelerated by heat. So it often manifests
itself as a "through-hole" problem, but this is usually because after
having gone through two reflow cycles and washes and dry-bakes, etc.,
the problem becomes so bad that hand-soldering becomes difficult. The
description of the problems they are having follows the classic pattern
of this type of issue.

But there are other issues that can lead to this, and they are similar
in nature. Nickel skips or nickel that is too thin, or gold that is too
thin to prevent the nickel underneath from oxidizing (flash gold
improperly deposited) are some other causes that come to mind. 
But those are not really ENIG as defined per the specification.



-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Jim Ma
Sent: Thursday, June 14, 2007 1:55 AM
To: [log in to unmask]
Subject: Re: [TN] ENIG Solderability

Hi Nancy:

    I think the shelf life is very importment for the solderability,
please make sure that the PCB w/ the vacuum package before opening, and
make sure that the time between the PCB opening to pre-reflow.

    From:Jim Ma

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2