Hi Blair,
Those devices are commercial grade (IPC class 1), planned to work up to
5 years.
The main issue (reason for failure such DOA) for Lead Free technology
(as mentioned in the laptop) is not the alloy but the small working /
process window in the production line such as:
1. Solderability / wetting problems (type of finish of each
component, short shelf life of PCBs finish etc.).
2. High peak profile temp (swelling, delamination, plastics
deformation).
The change of alloy is affecting the long term reliability and hi stress
conditions.
Best Regards
Reuven ROKAH
e mail: [log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Hogg, Blair K.
Sent: Wednesday, May 30, 2007 3:51 PM
To: [log in to unmask]
Subject: Re: [TN] RoHS compliant laptop with early failure
Doesn't Sony make the Playstations? We've got two in our house that have
been working since the day they came home. Only problem is that
scratched disks cause the kids don't put them back in the cases when
they are done with them.
Not that I'm a Sony fan...., but someone else makes the X-box.
I bought a 3 letter DVD/VCR combo player, it died within a year. Looking
for a digi-camcorder, won't buy that brand...
Blair
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.
Sent: Wednesday, May 30, 2007 8:38 AM
To: [log in to unmask]
Subject: Re: [TN] RoHS compliant laptop with early failure
My comments on this:
We purchased an X-box 360 for my son last Christmas. That is 5 months
ago.
The first one did not work out of the box.
The second one worked great for two weeks. Then the disk drive died.
The third replacement worked until yesterday, then the disk drive died.
My son reported to me that six other kids in his class have X-box 360s,
and every one of them failed and had to be returned at some point.
I do not know if the X-box is RoHS-compliant, or if they were soldered
with Pb-free solder.
I do know their quality is, in a single word, crap.
Like others, I had always expected better things from Sony. Not anymore.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Joe Fjelstad
Sent: Wednesday, May 30, 2007 12:14 AM
To: [log in to unmask]
Subject: Re: [TN] RoHS compliant laptop with early failure
Dear Inge,
Thank you for your note and thoughts. I greatly appreciate your sharing
them as you are a balanced thinker whose opinions i greatly respect. (I
hope I have not lost completely your confidence in my abilities to do
so... ;-)
My message was just a personal experience and I do not question that
there are "many trees still standing in the forest". I was simply
sharing an ironic event given my long standing opposition.
I have owned and/or used more than a dozen laptops in the last 17 years
and this is the most expensive one and the most hyped (in terms of
reliability) among them. It is also first one among them to have failed
without apparent cause.
I cannot predict the future but I can read and interpret scientific
data and indications are that we are looking at a very bumpy road
ahead. I listened to a talk by Dr. Fay Hua at a recent SMTA event and
it was very sobering.
The failure aside, my greatest frustration remains that the RoHS
products we are now being forced to buy are not as environmentally
friendly as the earlier products. Moreover, if we are to recycle, (which
I am in accord with) then the matter of lead in solder is moot.
Best wishes,
Joe
************************************** See what's free at
http://www.aol.com.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
*******************************************************************
This email and any files transmitted with it are confidential and
intended solely for the use of the individual or entity to whom they
are addressed. If you have received this email in error please notify
the system manager.
This footnote also confirms that this email message has been swept
for the presence of computer viruses.
www.Hubbell.com - Hubbell Incorporated
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|