Iain,
I look forward to hearing. I t is hard to believe that there we not a
high current arc on the burnt looking sample. The white or near white
could be something else like moisture. I have seen failures of the oxide
but they are not usually that even. If there are larger blisters and you
cut them open then catch the smell of ammonia that would be from moisture.
Are you X-sectioning?
Chuck Brummer
3M Manufacturing Engineer
8357 Canoga Ave.
Canoga Park, CA 91304-2605
(818) 734-4930
"Braddock, Iain" <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
05/09/2007 02:42 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
"Braddock, Iain" <[log in to unmask]>
To
[log in to unmask]
cc
Subject
Re: [TN] Strange one?
Chuck,
That was my comment to the Lab however they were adamant that wasn't the
case. The area under the blasted part on pic 1 was delaminated but due
to the surface of the Cu being etched away. They managed to replicate
the etched area on the Cu under the Polyimide and the fact it became
conductive by placing a spot of Alkaline on the board.
I will be checking another board with similar test fault though that
will not be until next week.I'll let you now the outcome.
Regards,
Iain.
________________________________
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: 08 May 2007 17:54
To: TechNet E-Mail Forum; Braddock, Iain
Subject: Re: [TN] Strange one?
*** WARNING ***
This mail has originated outside your organization,
either from an external partner or the Global Internet.
Keep this in mind if you answer this message.
Iian,
Stop fixing small shorts with your hi pot tester. Wow, Big flash and
the short is gone leaving you on pic 1 a delaminated area and on pic 2
the burnt remains.
Bet if you look real close you will find a sliver of metal or a copper
fiber.
Chuck Brummer
3M Manufacturing Engineer
8357 Canoga Ave.
Canoga Park, CA 91304-2605
(818) 734-4930
"Braddock, Iain" <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
05/08/2007 09:23 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
"Braddock, Iain" <[log in to unmask]>
To
[log in to unmask]
cc
Subject
[TN] Strange one?
Hi all,
Stevie G has been kind enough to post a couple of pics of a flexi
anomaly I've come across.
Been having problems with some flexi-rigid boards failing at Ins/Cons
test due to insulation breakdown - tested at 200v.
Had the lab do some exploratory work and the guys have come up with
these pics. along with the fact that the Polyimide was conductive
around the areas highlighted on the pics. but only localised. The Lab
view seems to be that something was left on the board during fabrication
and caused the problem; they have their suspicions but would like to
know if anyone else has encountered a similar problem.
http://stevezeva.homestead.com/files/Flex_Problem_1.JPG
<http://stevezeva.homestead.com/files/Flex_Problem_1.JPG>
http://stevezeva.homestead.com/files/Flex_Problem_2.JPG
<http://stevezeva.homestead.com/files/Flex_Problem_2.JPG>
Regards,
Iain.
********************************************************************
This email and any attachments are confidential to the intended
recipient and may also be privileged. If you are not the intended
recipient please delete it from your system and notify the sender. You
should not copy it or use it for any purpose nor disclose or distribute
its contents to any other person.
MBDA UK Limited, a company registered in England and Wales, registration
number 3144919 whose registered office is at Six Hills Way, Stevenage,
Hertfordshire, SG1 2DA, England.
********************************************************************
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|