Hi Miguel,
I have no problems with the first part of your recommendation:
> I would recommend a ramp-up (to 150 deg C)of 2-3 degC/sec and soak at about
> 150-160 deg C, for about 1.5 mins. then spike to reflow in about 30 secs.
>
The problem starts here:
> Stay at liquidous for about 45 secs
>
That does not mean very much and may be totally inadequate depending on your
assembly. To have assured good wetting, provided good solderability, the
slowest heating solder joint needs to be a Liquidus+20C for at least 5 seconds [all
other joints will be at higher T's for longer times]
Werner
**************************************
See what's free at http://www.aol.com.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------