TECHNET Archives

April 2007

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Edward Mines <[log in to unmask]>
Date:
Wed, 25 Apr 2007 11:50:09 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Subject:
From:
Joel Alexander <[log in to unmask]>
In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (87 lines)
IPC-CC-830 is a standard used by the manufacturer of the conformal coating 
to qualify their material. Can these also be applied to the application by 
the end user. IPC-A-610 states that bubbles are acceptable as long as they 
do not bridge adjacent conductors. 

Also is there a specific reference that states anything about the 
appearance of foam?



Joel Alexander
Quality Assurance Manager
TT APSCO, INC. 




Edward Mines <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
04/25/2007 10:26 AM

Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Edward Mines <[log in to unmask]>


To
[log in to unmask]
cc

Subject
[TN] bubbles in conformal coating






MIL-I-46058 & now IPC-CC-830 say conformal coatings should be "bubble 
free". Some have interpreted this as meaning that a few small bubbles away 
from components are acceptable.
  Foam is not acceptable.
 
  Some polyurethane conformal coatings generate gas as they cure. They 
should not be coated on very humid days. 
 
  Bubbles are also apt to form in conformal coatings when the coating is 
too thick. I've seen this happen in between closely spaced tall components 
even when the coating on most of the board is within customary limits and 
has no bubbles. The solution was to change the application technique.
 
  Get the coating and equipment manufacturers involved. They want your 
future business.
 
  Ed Mines

 
---------------------------------
Ahhh...imagining that irresistible "new car" smell?
 Check outnew cars at Yahoo! Autos.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------

ForwardSourceID:NT000B44EA 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2