TECHNET Archives

April 2007

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, ZLATKO BIJEDIC <[log in to unmask]>
Date:
Fri, 13 Apr 2007 19:38:03 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Lee parker <[log in to unmask]>
Subject:
From:
Lee parker <[log in to unmask]>
X-cc:
Tom Newton <[log in to unmask]>
Content-Transfer-Encoding:
7bit
Content-Type:
text/plain; charset="iso-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (177 lines)
Zlatko

Please contact Tom Newton at the IPC.

Best reguards

Lee

J. Lee Parker, Ph.D.
JLP Consultants LLC
804 779 3389


----- Original Message ----- 
From: "ZLATKO BIJEDIC" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Friday, April 13, 2007 6:06 PM
Subject: Re: [TN] Via hole plating corner crack


> Hi Mr. Parker:
>
> Could you please give me direction how I can get your paper you presented 
> at APEX.
> Regards
>
>
> ----- Original Message ----
> From: Lee parker <[log in to unmask]>
> To: [log in to unmask]
> Sent: Wednesday, April 11, 2007 12:41:40 PM
> Subject: Re: [TN] Via hole plating corner crack
>
>
> Victor
>
> You mentioned that the current density is 30 amps per square foot. I
> consider this to be extremely high and not only will cause brittle copper,
> but highly non-uniform copper in the barrel. I presented a paper at Apex
> that mathematically modeled the copper uniformity in the barrel to the
> plating parameters including current density, you might want to review 
> this
> paper. The model shows there is an inverse linear dependence between the
> copper uniformity and the plating density.
> Best regards
>
> Lee
>
> J. Lee Parker, Ph.D.
> JLP Consultants LLC
> 804 779 3389
> ----- Original Message ----- 
> From: "Victor G. Hernandez" <[log in to unmask]>
> To: <[log in to unmask]>
> Sent: Tuesday, April 10, 2007 10:36 AM
> Subject: Re: [TN] Via hole plating corner crack
>
>
>    Can you please post the crack via cross section photo for viewing, "a
> picture is worth one thousands words".   Is this SnPb or LF?
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of C J Long
> Sent: Tuesday, April 10, 2007 9:20 AM
> To: [log in to unmask]
> Subject: [TN] Via hole plating corner crack
>
> Dear Techneter:
>
> I recently experienced customer return of corner crack. The PCB is 50
> mil
> thick, 10 mil via, OSP finish and corner crack is over the 4 corners of
> top
> and bottom
> of hole. Crack is started from the bottom of external foil and crack
> through
>
> the entire plating. You can see the photo (file: crack through) of
> actual
> failure. Plating is unusual column type crystal on the surface. In the
> hole
> barrel, the plating crystal is regular. We also performed many in-procss
> WIP
>
> cross section (refer to the file "crack 9X IR") and we could only find
> the
> crack after 6X IR reflow and its crack is started from external foil top
> corner. I have sucessfuly duplicated similar failire with very high
> plating
> current density of 30ASF with very low brighter (0.15cc/l), but its
> failure
> mode is crack on ehe top of external foil not the same as customer
> return.
> My questions are:
>
> 1. Are these two failre modes with the same root cause? What is the
> reason
> one crack is started from the foil top corner and the other is from the
> bottom?
> 2.Is there any non-destructive method able screening the cracked
> plating?
>
>
> http://tw.pg.photos.yahoo.com/ph/minalong2003/album?.dir=/5c32scd
>
> Thank you very much.
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text
> in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at:
> http://listserv.ipc.org/archives
> Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
> ext.2815
> -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> ----------------------------------------------------- 
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to 
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to 
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
> for additional information, or contact Keach Sasamori at [log in to unmask] or 
> 847-615-7100 ext.2815
> -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to 
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to 
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
> for additional information, or contact Keach Sasamori at [log in to unmask] or 
> 847-615-7100 ext.2815
> -----------------------------------------------------
> 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2