Joel,
We use a moisture cure urethane and if we get the coating on too thick
and the humidity is high we get foam like bubbles. I believe the coating
skins over too fast trapping all the volatiles underneath. We resolved
this by doing a 40% first coat and then a 60% second coat to get the
required thickness. We only allow about 20 - 30 minutes between coats.
And like Ramon said, don't put them in an oven too soon after coating if
you oven dry your boards.
KennyB
-----Original Message-----
From: BADRI [mailto:[log in to unmask]]
Sent: Tuesday, April 24, 2007 6:15 AM
To: [log in to unmask]
Subject: Re: [TN] Conformal Coating Voids
I agree with Ramon. It is practically true.We solved the air bubble
issue by
placing the PCBA's in a closed box for an hour. This eliminated bubbles.
Since our qty of assembly is low we use a syringe to dispense the
coating
material. We also ensure that the syringe is full and has no entrapment.
Thanx
Badri
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Dehoyos, Ramon
Sent: Tuesday, April 24, 2007 6:23 PM
To: [log in to unmask]
Subject: Re: [TN] Conformal Coating Voids
Many of times bubbles are caused by the solvents warming up too
fast and turning into gas while still in the Coating. It could be too
fast air movement going over the coating while being coated or placing
the boards in the oven right away. In many instances the bubble are all
the way to the top of the surface of the coating. It is necessary to let
the board skin in a box for about 30 min prior to place them in an oven.
One way to fix the problem is to brush or spray the conformal coating
with one of the solvents in the coating and melting the bubbles out. Let
it skin and place the board in the oven. I would not fight the customer.
Experiment on one board with the advice from the coating manufacturer.
Show the way the board is and after the effort to the customer. Win the
battle and war and keep the customer happy. Good luck.
Ramon
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Hernefjord Ingemar
Sent: Tuesday, April 24, 2007 8:27 AM
To: [log in to unmask]
Subject: Re: [TN] Conformal Coating Voids
Brian,
The day you agree blindly on what I say, I will get worried, Brian.
Theoretically, you are so right, sir. But I dare use the conclusions of
daily work and practical experience. We accept single bubbles, air
entrapments or outgassing entrapments, according to what I said, but if
the bubbles increase in size, and become real atmospheric or gas bridges
between hot lines or between package leads, then we pull the emergency
brake and call people to MBR or similar. Our failure report system, as
well as incoming inspection and other tools, have not indicted one
single failure caused by \single\ bubbles in the coatings the last 20
years. At the same time, I take the occasion to mention about
globtopping or passivation or coating semi chips. Here, bubbles can be
catastrophic. But that belongs more or less to IMAP members and like, I
think. Naked semi chips on PWBs still not a hit, which I regret. COB
would make daily life little more interesting....
Thanks for your correct adds.
By the way, can you still find useful Cu on your isle
Inge
-----Original Message-----
From: Brian Ellis [mailto:[log in to unmask]]
Sent: den 24 april 2007 13:06
To: TechNet E-Mail Forum; Hernefjord Ingemar
Subject: Re: [TN] Conformal Coating Voids
I would disagree with your blind acceptation of isolated bubbles, Inge.
I would insist on knowing the cause of the bubbles before accepting
them, and their location. It would not be oxygen that would worry me;
have you thought about water vapour that could condense? Even if there
is only one now, will there be more in a few months?
Now, let's look at modern high-speed/frequency electronics. An airfilled
microbubble between a transmission line pair will have little effect
because substituting a dielectric constant of 1 for, say, 3 over such a
tiny distance will hardly cause a visible blip on your TD reflectometer.
But are you sure that a dielectric constant of 72, instead of 3, would
have so little effect? Not to mention the capacitive effect from
neighbouring tracks causing crosstalk?
And one little thought for you to ponder: all vesication probably starts
with a single microbubble.
Sorry to upset your complacency.
Brian
Hernefjord Ingemar wrote:
> If you get bubbles that 'look like foam', there is something wrong in
> the process. We use Humiseal acrylic coatings, and have tried Urethane
> before. Single microscopic bubbles are acceptable, which means in the
> range 1 mil or less. We use to say, that the bubbles must not exceed
> one third of the total thickness of the coating.
>
> A bubble is entrapped atmosphere, and the oxygen content can
> theoretically cause oxidation. The oxygen content in such little a
> bubble is not enough to cause any oxidation. When you use the word
> corrosion, one use to think of chemical reactions serious enough to
> damage the whole solder joint, or make the lead fall off the package.
> I would like to see the microscopic bubble that could cause such
damage!
> Would be no less than a miracle! Single air bubbles is nothing to be
> worried about, foam of bubbles is something you need overlook.
>
> Inge
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Joel Alexander
> Sent: den 23 april 2007 21:47
> To: [log in to unmask]
> Subject: [TN] Conformal Coating Voids
>
> We are using Urethane coating on an assembly that uses 63/37 solder.
> We are using organic water soluble flux. We are Ionic testing after
> wash and we are well within IPC cleanliness specifications. We
> installed a selective coating machine and in our initial run of
> product we had some small bubbles that look like foam. Our customer
> does not like it but our stand is that it meets IPC-A-610 and
> J-STD-001 requirements since there in no obvious voids between
> conductors. They were worried about corrosion if a bubble was against
> a lead. The bubbles are fully encapsulated. Does anyone think this is
a valid concern?
>
>
>
> Joel Alexander
> Quality Assurance Manager
> TT APSCO, INC.
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
> unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
> or
> (re-start) delivery of Technet send e-mail to [log in to unmask]: SET
> Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
> posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
> archives of previous posts at: http://listserv.ipc.org/archives Please
> visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at
> [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
> unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
> or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET
> Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
> posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
> archives of previous posts at: http://listserv.ipc.org/archives Please
> visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at
> [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or
847-615-7100 ext.2815
-----------------------------------------------------
Disclaimer:
===========
This E-mail may contain privileged information and is intended solely
for the addressee. Any unauthorized use or dissemination of this message
in whole or in part is strictly prohibited. If you have received this
mail by mistake, please inform us immediately and delete this mail. Any
information expressed in this mail does not necessarily reflect the
views of Avalon Technologies (P) Ltd .
Avalon Technologies(P) Ltd shall not be responsible nor liable for the
proper and complete transmission of the information contained in this
communication nor for any delay in its receipt or damage to your system.
Avalon Technologies(P) Ltd does not guarantee that the integrity of this
communication has been maintained nor that this communication is free of
interceptions or interference.We have taken precautions to minimize the
risk of transmitting software viruses, but we advise you to carry out
your own virus checks on any attachment to this message. We cannot
accept liability for any loss or damage caused by software viruses.
Thank you for your cooperation
AVALON TECHNOLOGIES MAY MONITOR ALL INCOMING AND OUTGOING MAILS.
************************************************************************
************************************************************************
************************************************************************
************************************************************************
************************************************************************
************************************************************************
************************************************************************
************************************************************************
************************************************************************
************************************************************************
*************************************************************
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|