James, Indium Corporation does not recommend using a high Sn alloy, such as
Sn96, with gold plating due to the brittle Au/Sn intermetallics that could
form and cause reliability issues. However it depends on the thickness of
the gold layer. Typically if you have 10-15 micro-inches of gold the gold
will act as a sacrificial layer. This gold layer will protect the nickel
from oxidation and will dissolve into the solder joint and you will actually
be soldering to the nickel or underlying metallization. If you have 40-50
micro-inches, or more, gold you are actually soldering directly to the gold
instead of the underlying metallization. The Sn will scavenge the gold and
will form brittle Au/Sn intermetallics. I believe the industry is agreeing
that 3% gold by weight, in a joint, is an acceptable amount of gold that
will not cause any brittle Au/Sn intermetallic formation. The major concern
here is long term reliability.
Christopher J. Nash
Mid-West Technical Support Engineer
Indium Corporation of America
Phone #: (315) 853-4900 x7521
Fax #: (315) 853-1000
www.indium.com
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Marsico, James
Sent: Friday, March 30, 2007 8:21 AM
To: [log in to unmask]
Subject: Re: [TN] Soldering using Sn96
http://www.microwaves101.com/encyclopedia/solderchart.cfm
Go to the chart and see alloy 96.5Sn 3.5Ag
Jim Marsico
EDO Corporation
1250 New Horizons Blvd.
North Amityville, NY 11701
631-630-5079
[log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Donald Kyle
Sent: Friday, March 30, 2007 8:12 AM
To: [log in to unmask]
Subject: Re: [TN] Soldering using Sn96
Good morning Jim,
Do you have an URL for this CHART that we can look at?
For me Sn96 and gold works like a hose.
Donald Kyle
At 06:58 AM 3/30/2007, you wrote:
>Mornin' Jim!
>
>Really? That's strange...almost every downhole assembly that I've built
>has always been with ENIG plated PCB's...
>
>-Steve Gregory-
>
>-----Original Message-----
>From: TechNet [mailto:[log in to unmask]] On Behalf Of Marsico, James
>Sent: Friday, March 30, 2007 6:46 AM
>To: [log in to unmask]
>Subject: [TN] Soldering using Sn96
>
>Technetters:
>
>
>
>I happened to come across a solder chart from the Indium Corporation
and
>noticed that they do not recommend using Sn96 solder on gold-plated
>surfaces. Can anyone elaborate on this?
>
>
>
>Jim Marsico
>
>EDO Corporation
>
>1250 New Horizons Blvd.
>
>North Amityville, NY 11701
>
>631-630-5079
>
>[log in to unmask]
>
>
>
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
>unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
or
>(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
>Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
>posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
>archives of previous posts at: http://listserv.ipc.org/archives Please
>visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
>additional information, or contact Keach Sasamori at [log in to unmask] or
>847-615-7100 ext.2815
>-----------------------------------------------------
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0
>To unsubscribe, send a message to [log in to unmask] with following text
in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at:
http://listserv.ipc.org/archives
>Please visit IPC web site
>http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
>information, or contact Keach Sasamori at [log in to unmask] or
>847-615-7100 ext.2815
>-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
***This email, its content and any files transmitted with it are intended solely for the addressee(s) and may be legally privileged and/or confidential. If you are not the intended recipient please delete and contact the sender by return and delete the material from any computer. Any review, retransmission, dissemination or other use of, or taking of any action in reliance upon, this information by persons or entities other than the intended recipient is prohibited.
Messages sent via this medium may be subject to delays, non-delivery and unauthorized alteration. This email has been prepared using information believed by the author to be reliable and accurate, but Indium Corporation makes no warranty as to accuracy or completeness. In particular, Indium Corporation does not accept responsibility for changes made to this email after it was sent. Any opinions or recommendations expressed herein are solely those of the author. They may be subject to change without notice.***
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|