Hello Ioan,
I saw a similar concern over 10 years ago so I am using my memory on
this.
See the answer below:
Your question is: when reflowing the second side, the one that requires
>lower temps because the components are less demanding, may the reflow
>recipe be colder? Will this affect the other side, that will reflow
again,
>but at lower temps and for not as long? I mean the IMC is already
formed;
>is there anything else that could go wrong?
You have 2 conditions in this scenario:
1- When reflowing the second side (with small parts) you will also
reflow the component solder joint from the first side (with large
parts). In this case they will fall off the PCB and you do not have a
product.
2- Somehow, when reflowing the second side (with small parts) you will
not reflow the component solder joints from the first side (with large
parts). In this case, from my memory from many years ago, the IMC will
grow at a high rate. I remember that the most growth would take place at
160C to 180C before the solder reaches its eutectic reflow temp.
So if you need to evaluate this condition, then setup your process,
measure the solder joint temperatures for the components from the first
side during the reflow profile for the second side. Then approach our
industry reliability experts to provide you with their comments about
the reliability of these solder joints.
Hope this helps,
Paymon Sani
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Tempea, Ioan
Sent: March 28, 2007 4:13 PM
To: [log in to unmask]
Subject: Re: [TN] Double sided reflow
Phil,
you are right if we consider a somewhat balanced top-bottom component
distribution.
What I am talking about is the case where the heavy stuf, BGAs,
heatsinks, transformers, etc, are all on the first side that is
soldered, whereas on the second side there are small discretes only,
e.g. 0603 and 1206. In this case you can solder the discretes at lower
temperatures, but these temperatures are not enough to properly reflow
the joints of the first side.
Don't ask me why would I do such a stupid thing, reflow the havily
loaded side before the light one. I am simply trying to brainstorm on
how to reduce setup times at the reflow oven. And the basic rule of
brainstorming says that nothing is stupid a priori.
Thanks,
Ioan
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Phillip Bavaro
Sent: Wednesday, March 28, 2007 3:45 PM
To: [log in to unmask]
Subject: Re: [TN] Double sided reflow
Ioan,
Someone can't see the forest because the trees are in the way....lol.
The second side reflow is actually more thermally demanding because it
has
to account for both sides of the board with respect to mass. Set your
reflow profile up for the double sided reflow only and use it for both
sides.
Phil
At 03:42 PM 3/27/2007 -0400, Tempea, Ioan wrote:
>Dear colleagues,
>
>let's take a board with SMT on both sides. Let's say that for
particular
>reasons we have to solder the more thermally demanding side first.
>
>The question is: when reflowing the second side, the one that requires
>lower temps because the components are less demanding, may the reflow
>recipe be colder? Will this affect the other side, that will reflow
again,
>but at lower temps and for not as long? I mean the IMC is already
formed;
>is there anything else that could go wrong?
>
>Or, to generalize, a PCB with SMT parts that were properly reflowed
once,
>can it be reflowed again at lower temperatures, without adverse effects
on
>the metallurgy of the joints?
>
>Thanks for your help,
>
>Ioan
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0
>To unsubscribe, send a message to [log in to unmask] with following text
in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at:
http://listserv.ipc.org/archives
>Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>for additional information, or contact Keach Sasamori at [log in to unmask]
or
>847-615-7100 ext.2815
>-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------------------------------------------
Confidentiality Notice
This e-mail and any attachment(s) are intended for the individual or entity to which this email is addressed and may contain information that is confidential. If you are not the intended recipient or an employee or agent responsible for delivering this e-mail to the intended recipient, please be aware that any dissemination, distribution or copying of this communication is strictly prohibited. If you have received this in error, please notify the sender by telephone at 604.430.4336 or by return e-mail, and please delete or destroy all copies of this communication. Thank you!
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|