Paymon Sani:
The problem is probably caused by the catalyst in the ENIG absorbing into the soldermask, and FR-4.
Not an unknown problem in the ENIG process.
An immediate help may be to reduce the time, or metal content in the catalyst.
A permenant solution would be to change to another catalyst.
We offer a catalyst specifically designed to make this problem go away.
Rudy Sedlak
RD Chemical Company
Paymon Sani <[log in to unmask]> wrote: Hello All,
I have noticed a trend with our ENIG PCBs where Nickel is growing beyond
the Copper and onto the FR4 and Soldermask. I would like to know:
* Is it a cause for concern with our assembly process?
* Is it a cause for concern for the end user?
* How is it caused?
* How could it be prevented?
If you know the answers to any of the above I would appreciate your
feedback.
Cheers,
Paymon
---------------------------------------------------------------------------------------
Confidentiality Notice
This e-mail and any attachment(s) are intended for the individual or entity to which this email is addressed and may contain information that is confidential. If you are not the intended recipient or an employee or agent responsible for delivering this e-mail to the intended recipient, please be aware that any dissemination, distribution or copying of this communication is strictly prohibited. If you have received this in error, please notify the sender by telephone at 604.430.4336 or by return e-mail, and please delete or destroy all copies of this communication. Thank you!
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------
Now that's room service! Choose from over 150,000 hotels
in 45,000 destinations on Yahoo! Travel to find your fit.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|