Did you try turning the convection blowers down a bit? We noticed that
tombstones increase if you are just on the edge of moving the parts.
O508s do have a bigger terminal, and shorter rotation to tombstone.
You might also try a thinner stencil.
Smaller paste deposit. Bow Tie pattern . . . or combination. You need to
weaken the force enough to stop lifting the part.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Dehoyos, Ramon
Sent: Monday, January 15, 2007 2:24 PM
To: [log in to unmask]
Subject: Re: [TN] tombstoning of 0508 ceramic capacitors
Hi Royce:
Have you tried two smaller dots of adhesive instead of
one larger one? The same amount of glue would be dispensed but along
the width of the part.
Regards,
Ramon
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Royce Taylor
Sent: Monday, January 15, 2007 2:04 PM
To: [log in to unmask]
Subject: [TN] tombstoning of 0508 ceramic capacitors
I have a question for the "Adhesive Dispense" OR the "0508 chip"
experts out in Technet land.
We at times struggle with 0508 capacitors tombstoning (yes, 0508 not
0805). We do run Nitrogen and turning it off helps at times but there
are many times we need to run nitrogen for other reasons. Most times we
try to dispense a dot of adhesive (Loctite 3609) but we are having
occasional issues with the adhesive getting into the solderpaste, the
gap between the pads measures ONLY 0.020" so it is difficult to prevent
this from happening. Does anyone out there run into the same issues??
Any thoughts?? We run a Camalot Gemini and a Fuji GL dispenser and use a
25 GA needle. Also we use Indium SMQ92J No Clean solderpaste so I don't
know if this paste is contributing to the tombstoning.
A re-layout of the boards is not an option. We have tried both a
"straight ramp" and a "ramp-soak-ramp" profile with little or no
difference.
Thanks for your thoughts and advice
Royce
*************************************************
Royce Taylor
Raytheon
350 Lowell St.
Andover, MA 01810
(978) 470-7431
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|