Steve and Bill: I've seen this when the wrong solvent i.e.
thinner/reducing agent was added to the soldermask to adjust viscosity
prior to application. If you add a solvent with the wrong (lower)
boiling point, when you tack dry or B-stage the mask it outgases too
rapidly forming pinhole eruptions.
It usually occurs when an operator is out of the correct solvent and
adds whatever is "in the cabinet" to adjust the viscosity.
Regards
Michael Barmuta
Staff Engineer
Fluke Corp.
Everett WA
425-446-6076
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: Wednesday, December 06, 2006 12:44 PM
To: [log in to unmask]
Subject: Re: [TN] Pock marks in the soldermask??
Hi Bill!
I got your pictures and put them in a *.doc file. They are here:
http://stevezeva.homestead.com/files/Mask.doc
They look like pin-holes to me. Here's a trouble-shooting guide for
LPI's from Enthone for their mask:
http://www.enthone.com/docs/Imup9.pdf
Maybe one of those causes?
-Steve Gregory-
________________________________
From: Brooks,Bill [mailto:[log in to unmask]]
Sent: Wednesday, December 06, 2006 1:56 PM
To: Steve Gregory
Subject: FW: Pock marks in the soldermask??
-----Original Message-----
From: Brooks,Bill
Sent: Wednesday, December 06, 2006 11:54 AM
To: [log in to unmask]
Subject: FW: Pock marks in the soldermask??
Here are the pics
Bill Brooks
PCB Design Engineer, C.I.D.+
Tel: (760)597-1500 Fax: (760)597-1510
Datron World Communications, Inc.
Vista, California
-----Original Message-----
From: Brooks,Bill
Sent: Tuesday, December 05, 2006 12:37 PM
To: 'TechNet E-Mail Forum'
Cc: [log in to unmask]
Subject: Pock marks in the soldermask??
I'm sending some pictures of what we think is an odd soldermask
defect...
Can someone help me identify or at least speculate on the specific cause
of this strange effect?
Bill Brooks
PCB Design Engineer, C.I.D.+
Tel: (760)597-1500 Fax: (760)597-1510
Datron World Communications, Inc.
Vista, California
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
This message (including any attachments) contains confidential
and/or proprietary information intended only for the addressee.
Any unauthorized disclosure, copying, distribution or reliance on
the contents of this information is strictly prohibited and may
constitute a violation of law. If you are not the intended
recipient, please notify the sender immediately by responding to
this e-mail, and delete the message from your system. If you
have any questions about this e-mail please notify the sender
immediately.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|