Slowing the board travel through the WS, top and bottom fluxing,
preheating ground plane/thick boards improves PTH solder penetration.
Ramon
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Mike Fenner
Sent: Friday, December 01, 2006 3:29 AM
To: [log in to unmask]
Subject: Re: [TN] Solder Voids in Hole barrel after W/S
Assuming you have adequate top and bottom preheating the cause is almost
certainly poor PCB fabrication. You could try baking out the boards
before soldering to see if this has an effect on the incidence/severity.
This won't cure the problem but a change will point to the cause.
Regards
Mike Fenner
Indium Corporation
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Irving Lee
Sent: Thursday, November 30, 2006 4:31 PM
To: [log in to unmask]
Subject: [TN] Solder Voids in Hole barrel after W/S
What are the critical control factors to avoid solder voids in hole
barrel after W/S ?
We have checked following items , but still have serious solder void
problem .
1. Good Hole Wall Quality
2. Good solderability for component tail 3. Good HASL thickness 4. No
Ionic contamination
Irving Lee
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
-----------------------------------------------------
***This email, its content and any files transmitted with it are
intended solely for the addressee(s) and may be legally privileged
and/or confidential. If you are not the intended recipient please delete
and contact the sender by return and delete the material from any
computer. Any review, retransmission, dissemination or other use of, or
taking of any action in reliance upon, this information by persons or
entities other than the intended recipient is prohibited.
Messages sent via this medium may be subject to delays, non-delivery and
unauthorized alteration. This email has been prepared using information
believed by the author to be reliable and accurate, but Indium
Corporation makes no warranty as to accuracy or completeness. In
particular, Indium Corporation does not accept responsibility for
changes made to this email after it was sent. Any opinions or
recommendations expressed herein are solely those of the author. They
may be subject to change without notice.***
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|