I echo your comment about this not being an immersion sil
Denny,
I echo your comment about this not being an immersion silver problem.
We've seen these types of defects, fortunately very infrequently, and
they are usually associated with imaging issues. If there is an
appropriate amount of copper in the PTH's the amount of copper consumed
during a replacement reaction that deposits only a few microinches of
silver should not etch enough copper to cause the ring voids.
Regards,
George
George M. Wenger
Andrew Corporation Wireless Network Solutions
Senior Principal FMA / Reliability Engineer
40 Technology Drive, Warren, NJ 07059
(908) 546-4531 [Office] (732) 309-8964 [Cell]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Dennis Fritz
Sent: Friday, December 15, 2006 3:38 PM
To: [log in to unmask]
Subject: Re: [TN] How does this happen?
In a message dated 12/15/2006 8:59:36 A.M. Eastern Standard Time,
[log in to unmask] writes:
Another possibility is that the single panel was reworked through
immersion silver. Immersion silver is notorious for etching copper as
it plates. I've seen it lift narrow traces right off the substrate.
The voids probably just correspond to naturally low areas of copper
plating, whether from PTH or electrolytic copper.
**************************
I still vote for an imaging problem and rework (maybe more than once) at
that step. There is nearly breakout of the surface pad at the 2:00
position of
the holes. I am 99.9% sure this is NOT an immersion silver problem -
first,
the fine trace is OK, and second, the small hole appears fine. Any
silver
attack problem is usually associated with an electrochemical cell set
up
between large copper and small copper areas (fine traces). These sort
of
"electrochemical cells" have been shown for years - such as where 0.5
ounce inner
layers in holes are recessively etched, compared to adjacent 2 ounce
inner
layers in MLB holes.
Denny Fritz
MacDermid, Inc.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
------------------------------------------------------------------------------------------------
This message is for the designated recipient only and may
contain privileged, proprietary, or otherwise private information.
If you have received it in error, please notify the sender
immediately and delete the original. Any unauthorized use of
this email is prohibited.
------------------------------------------------------------------------------------------------
[mf2]
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|