It happens. :-)
From the picture it looks like not thick enough layer of solder may be
present on the solder pad. Combining it with what George has said in his
e-mail and possible warpage of the board/package you well could get
something like those joints. If that is the case, then it can be
minimized by tweaking the re-flow profile. I read a paper somewhere on
the topic just a few months ago. I'll try to find it.
Regards,
Vladimir
-----Original Message-----
From: Leadfree [mailto:[log in to unmask]] On Behalf Of Tempea, Ioan
Sent: Wednesday, November 15, 2006 11:25 AM
To: [log in to unmask]
Subject: Re: [LF] [TN] Separation in BGA joints
Sorry Vladimir,
I haven't got your reply. Damn firewall...
Please see http://www.plxtech.com/support/packaging/9056bga.asp
Thanks,
Ioan
-----Original Message-----
From: Vladimir Igoshev [mailto:[log in to unmask]]
Sent: Wednesday, November 15, 2006 11:05 AM
To: (Leadfree Electronics Assembly Forum); Tempea, Ioan
Subject: RE: [LF] [TN] Separation in BGA joints
Ioan,
It could be board/package warpage during re-flow. Or contamination of
the bottom of the balls. That is why I asked you about the original ball
size.
Regards,
Vladimir
-----Original Message-----
From: Leadfree [mailto:[log in to unmask]] On Behalf Of Tempea, Ioan
Sent: Wednesday, November 15, 2006 10:58 AM
To: [log in to unmask]
Subject: Re: [LF] [TN] Separation in BGA joints
George, Victor,
foot-in-the-mud, head-on-pillow. It seems that you two are talking about
the same thing, but what is it and why is this happening?
The stencil is 6 mils thick with square apertures, the dimension equal
to the diameter of the pad. ENIG finish.
Time above liquidous is 65s.
Due to pressures from our customers we run many lead-free BGAs on leaded
paste at 220C. If this forms joints, why LF on LF would not form joints
at 246C, or let's say 230C if I am really off in my temp measurements?
Thanks,
Ioan
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Tempea, Ioan
Sent: Wednesday, November 15, 2006 9:57 AM
To: [log in to unmask]
Subject: [TN] Separation in BGA joints
Hi TNLF-ers,
please have a look at http://stevezeva.homestead.com/files/Ioan_Ball.jpg
, many thanks to Steve again.
What can I tell you: no-clean SAC305 at the bottom, the balls read a
sort of SAC with 3%Ag and 1.75%Cu
The reflow profile seems to be OK, I measure 246C under the periphery of
the BGA, with a thermocouple that is squeezed there. I know it is not
rigorous, I did not drill, I am not measuring inside the joint. But even
if I am 20C off, the materials should be molten and coalesce, isn't it?
The intermetallics solder paste - PCB pad are OK, the wetting is good,
the BGA balls seem to have changed shape, they are almost collapsed,
there is physical contact between the balls and the paste, but no joint.
The question is: why do I see the separation line? What can cause that?
Should I bother investigating the process, or do I have a sort of
contamination? Or the BGA ball alloy has a higher melting point?
Thanks,
Ioan
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
------------------------------------------------------------------------
-------Leadfee Mail List provided as a service by IPC using LISTSERV
1.8d
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Leadfree
To temporarily stop/(start) delivery of Leadree for vacation breaks
send: SET Leadfree NOMAIL/(MAIL)
Search previous postings at: http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
------------------------------------------------------------------------
-------
------------------------------------------------------------------------
-------Leadfee Mail List provided as a service by IPC using LISTSERV
1.8d
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Leadfree
To temporarily stop/(start) delivery of Leadree for vacation breaks
send: SET Leadfree NOMAIL/(MAIL)
Search previous postings at: http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
------------------------------------------------------------------------
-------
-------------------------------------------------------------------------------Leadfee Mail List provided as a service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Leadfree
To temporarily stop/(start) delivery of Leadree for vacation breaks send: SET Leadfree NOMAIL/(MAIL)
Search previous postings at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-------------------------------------------------------------------------------
|