TECHNET Archives

October 2006

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Hfjord <[log in to unmask]>
Date:
Fri, 6 Oct 2006 12:02:07 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Linda Langley <[log in to unmask]>
Subject:
From:
Linda Langley <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
<004301c6e8b4$d9157fe0$6401a8c0@compaq>
Content-Type:
text/plain; charset=iso-8859-1
MIME-Version:
1.0
Parts/Attachments:
text/plain (208 lines)
Has any one tried the Hakko FT 700 Tip Cleaner? Works great!

Linda

 -----Original Message-----
From:   TechNet [mailto:[log in to unmask]]  On Behalf Of Hfjord
Sent:   Thursday, October 05, 2006 3:31 PM
To:     [log in to unmask]
Subject:        Re: [TN] Solder iron question

Place
solder paste in a covered container. Open container and dipped the tip.
It comes out clean and shiny.

My granpa used to do that when I was a little boy, decades ago. He teached
me how to solder even stainless steel.
Oldies knew already.

Inge




----- Original Message -----
From: "Dehoyos, Ramon" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Thursday, October 05, 2006 8:16 PM
Subject: Re: [TN] Solder iron question


        I agree, the tip tinners are not liked by the operators here
neither. We also have the Hakko 599B tip cleaner, it works well.
Something else that I have tried and works well is solder paste. Place
solder paste in a covered container. Open container and dipped the tip.
It comes out clean and shiny.
        Ramon

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: Thursday, October 05, 2006 1:21 PM
To: [log in to unmask]
Subject: Re: [TN] Solder iron question

Speaking of Tip Tinners, I'm trying to discourage their use. I don't
think they're very good for solder tips over the long term, and may
actually lessen their useful life. Anybody else share my view?

What I've been buying for my operators to replace the little cans of tip
tinner is a Hakko 599B Tip Cleaner:

http://shop.kiesub.com/stores/Kiesub/catalog/hakko-599.jpg

It's a bit more abrasive than a sponge and really cleans the tips well,
including the baked on flux residues that build-up on the tips. I've had
nothing but positive comments from my operators.

-Steve Gregory-



-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: Thursday, October 05, 2006 11:12 AM
To: [log in to unmask]
Subject: Re: [TN] Solder iron question

Hi Gloria! I recommend your conduct two analytical tests if possible:
(1) an FTIR test to try to match the black residue to either your flux
or tinner; (2) SEM test to see if the black residue is comprised of
metal oxides. Have you tested to see if the 270WR and the tinner are
compatible with each other? Good Luck.

Dave Hillman
Rockwell Collins
[log in to unmask]




             Gloria Brown
             <gloriab@BURTONIN
             DUSTRIES.COM>
To
             Sent by: TechNet          [log in to unmask]
             <[log in to unmask]>
cc


Subject
             10/05/2006 08:34          [TN] Solder iron question
             AM


             Please respond to
             gloriab@burtonind
                ustries.com






Good Morning,



I need some information if available.  I am finding on our lead free
solder irons that there is a black substance that is rising up the
soldering shaft.
We are currently using an Aim 270WR flux, SN100C LF Solder, LF tinner,
Solder iron temp is 720, they are WD1 solder irons.



Can anyone give me some information on what this black substance may be?



Thanks



Gloria

phone 906-932-5970  ext. 26

fax  906-932-9822

[log in to unmask]




---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2