Why were they using SAC HASL? And what kinds of defects did you see?
-----Original Message-----
From: Leadfree [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: Thursday, September 21, 2006 8:21 AM
To: [log in to unmask]
Subject: Re: [LF] Galvanized RoHS & ENIG Finish
We just had some boards that came in here that were HASL'ed with a SAC
solder...they soldered like like crap. If I had a choice, I would use
ImAg...
-Steve Gregory-
-----Original Message-----
From: Leadfree [mailto:[log in to unmask]] On Behalf Of Peter Lymn
Sent: Thursday, September 21, 2006 8:04 AM
To: [log in to unmask]
Subject: Re: [LF] Galvanized RoHS & ENIG Finish
HASL is RoHS compliant. You only need to change the alloy used.
-----Original Message-----
From: Leadfree [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.
Sent: 21 September 2006 13:52
To: [log in to unmask]
Subject: Re: [LF] Galvanized RoHS & ENIG Finish
All surface finishes except HASL are RoHS compliant. I would strongly
recommend you do not convert your finishes to ENIG. Look at the postings
for the last two or three days to see examples of why not.
-----Original Message-----
From: Leadfree [mailto:[log in to unmask]] On Behalf Of Index Bruce Bryla
Sent: Thursday, September 21, 2006 6:26 AM
To: [log in to unmask]
Subject: Re: [LF] Galvanized RoHS & ENIG Finish
Good morning fellow Tec netters, first and foremost thank you all for
sharing your comments, experience and information. I have two questions.
1) Is an ENIG finish RoHS compliant or is its compliancy based on the
formula and / or process related?
We are looking at converting all our board finishes to ENIG to comply
with RoHS but in my research I can not locate any data that emphatically
states this finish is compliant. Many organizations that offer RoHS
alternatives list ENIG as an option.
2) I have been informed that passivation is RoHS compliant but have read
different opinion's as far as compliancy?
Any help would be greatly appreciated.
Bruce Bryla
-----Original Message-----
From: Leadfree [mailto:[log in to unmask]] On Behalf Of Brian Ellis
Sent: Thursday, September 21, 2006 2:56 AM
To: [log in to unmask]
Subject: Re: [LF] Galvanized RoHS
Ah! But that is the American Galvanizers Association. What does the
European Galvanisers Association (or whatever they call themselves) say?
:-D
Brian
Tempea, Ioan wrote:
> John and John,
>
> one of our suppliers sent this paper, to justify the lead we are
> finding with the XRF machine. I will try to find where did they get it
> from, in the mean time, the only thing I know is that it has been
> written by the American Galvanizers Association.
>
> Regards,
>
> Ioan
>
> -----Original Message-----
> From: Leadfree [mailto:[log in to unmask]]On Behalf Of John R. Sieber
> Sent: Wednesday, September 20, 2006 1:09 PM
> To: [log in to unmask]
> Subject: Re: [LF] Galvanized RoHS
>
>
> Ioan,
>
> Where can I find this paper on testing coated galvanized steel for
> RoHS compliance?
>
> My understanding is that some steel applications use sheet metal with
> two coatings on it. The first coating is a Zn or Zn-Al alloy applied
> by either a galvanic or a hot-dip process. The second, outer coating
> is the chromate process. [Can chromite process be substituted?] If
> you obtain a depth profile of this multi-layer structure you see a
> blurring of the interfaces between materials. At the surface, there
> is carbonaceous matter. Underneath that is the Cr-bearing layer which
> gradually incorporates Zn (and Al if present) as it morphs into the
> galvanic or hot-dip coating. Deeper yet, the Zn or ZnAl layer
> increases in Fe content as it transitions into the surface of the
> steel. The extent of intermixing depends on whether there was an
> annealing step included prior to the application of the Cr coating.
> None of the layer boundaries are sharp and all contain other elements
> either as contaminants or as alloy constituents. In addition, none of
> the layers are uniform in thickness and composition across the entire
> area of the sheet metal.
>
> This description is meant to impress on you that coatings are ugly
> beasts that make terrible analytical specimens. Probably many of you
> already know this. From the perspective of an analytical chemist,
> there is nothing homogeneous about them. Depth profiles have been
> obtained using glow-discharge atomic emission spectrometry, which does
> not tell you the oxidation state of the Cr. One can probably study
> the outer Cr-containing coatings using X-ray photoelectron
> spectrometry and other microanalysis techniques. I'd be surprised if
> very many coatings companies have these techniques available for
> manufacturing QA.
>
> regards,
>
> John Sieber
>
>
> At 12:34 PM 9/20/2006, you wrote:
>> The galvanised coat is not homogeneous with the steel in respect of
>> the RoHS definition of homogeneous. If it were then no one would be
>> worrying about all the other plated finishes!!
>>
>> Regards,
>>
>> Chris
>>
>>
>> -----Original Message-----
>> From: Leadfree [mailto:[log in to unmask]] On Behalf Of Tempea, Ioan
>> Sent: 20 September 2006 17:20
>> To: [log in to unmask]
>> Subject: [LF] Galvanized RoHS
>>
>> Hi everybody,
>>
>> Steve has been kind enough to post a document I have sent to him. The
>> paper practically says that galvanized steel is not considered a
>> coated structure, therefore the homogeneous material take on
>> galvanized steel considers the base material and coating to be one
>> element.
>>
>> What do you think about this?
>>
>> Thanks,
>>
>> Ioan
>>
>> ---------------------------------------------------------------------
>> ---
>> -------Leadfee Mail List provided as a service by IPC using LISTSERV
>> 1.8d To unsubscribe, send a message to [log in to unmask] with
>> following text in the BODY (NOT the subject field): SIGNOFF Leadfree
>> To temporarily stop/(start) delivery of Leadree for vacation breaks
>> send: SET Leadfree NOMAIL/(MAIL)
>> Search previous postings at: http://listserv.ipc.org/archives Please
>> visit IPC web site
>> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
>> information, or contact Keach Sasamori at [log in to unmask] or
>> 847-615-7100
>> ext.2815
>> ---------------------------------------------------------------------
>> ---
>> -------
>>
>> -----------------------------------------
>> This message (including any attachments) may contain confidential
>> information intended for a specific individual and purpose. If you
>> are not the intended recipient, delete this message. If you are not
>> the intended recipient, disclosing, copying, distributing, or taking
>> any action based on this message is strictly prohibited.
>>
>>
>> ---------------------------------------------------------------------
>> ----------Leadfee
>> Mail List provided as a service by IPC using LISTSERV 1.8d To
>> unsubscribe, send a message to [log in to unmask] with following text
>> in the BODY (NOT the subject field): SIGNOFF Leadfree To temporarily
>> stop/(start) delivery of Leadree for vacation breaks
>> send: SET Leadfree NOMAIL/(MAIL)
>> Search previous postings at: http://listserv.ipc.org/archives Please
>> visit IPC web site
>> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
>> information, or contact Keach Sasamori at [log in to unmask] or
>> 847-615-7100 ext.2815
>>
------------------------------------------------------------------------
----
---
>
> John R. Sieber, PhD
> Research Chemist
>
> National Institute of Standards and Technology Chemical Science and
> Technology Laboratory Analytical Chemistry Division 100 Bureau Drive,
> Stop 8391 Gaithersburg, MD 20899-8391 USA
>
> [log in to unmask]
> Tel: 1.301.975.3920
> Fax: 1.301.869.0413
> www.cstl.nist.gov/
>
> Identification of commercial items in this document does not imply
> endorsement by NIST or that items are
>
> ----------------------------------------------------------------------
> ---------Leadfee Mail List provided as a service by IPC using LISTSERV
> 1.8d To unsubscribe, send a message to [log in to unmask] with following
> text in the BODY (NOT the subject field): SIGNOFF Leadfree To
> temporarily stop/(start) delivery of Leadree for vacation breaks send:
> SET Leadfree NOMAIL/(MAIL) Search previous postings at:
> http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
>
------------------------------------------------------------------------
----
---
> necessarily the best for the purpose stated.
>
> ----------------------------------------------------------------------
> ---------Leadfee Mail List provided as a service by IPC using LISTSERV
> 1.8d To unsubscribe, send a message to [log in to unmask] with following
> text in the BODY (NOT the subject field): SIGNOFF Leadfree To
> temporarily stop/(start) delivery of Leadree for vacation breaks send:
> SET Leadfree NOMAIL/(MAIL) Search previous postings at:
> http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
>
------------------------------------------------------------------------
----
---
>
--
http://www.cypenv.org Cyprus environment/energy
http://www.cypenv.org/worldenv World environment/energy
http://www.cypenv.org/weather Cyprus weather
http://www.cypenv.org/smf/index.php Environment/energy forums
http://groups.yahoo.com/group/cypnature/ Cyprus nature forum
------------------------------------------------------------------------
----
---Leadfee Mail List provided as a service by IPC using LISTSERV 1.8d To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Leadfree To temporarily
stop/(start) delivery of Leadree for vacation breaks send: SET Leadfree
NOMAIL/(MAIL) Search previous postings at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
------------------------------------------------------------------------
----
---
This e-mail and subsequent attachments may contain information which is
proprietary to L-3 Communications Corporation. The contents shall not be
disclosed, copied, distributed or used unless authorized by L-3
Communications Narda - East.
------------------------------------------------------------------------
-------Leadfee Mail List provided as a service by IPC using LISTSERV
1.8d To unsubscribe, send a message to [log in to unmask] with following
text in the BODY (NOT the subject field): SIGNOFF Leadfree To
temporarily stop/(start) delivery of Leadree for vacation breaks send:
SET Leadfree NOMAIL/(MAIL) Search previous postings at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
------------------------------------------------------------------------
-------
------------------------------------------------------------------------
----
---Leadfee Mail List provided as a service by IPC using LISTSERV 1.8d To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Leadfree To temporarily
stop/(start) delivery of Leadree for vacation breaks send: SET Leadfree
NOMAIL/(MAIL) Search previous postings at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
------------------------------------------------------------------------
----
---
------------------------------------------------------------------------
-------Leadfee Mail List provided as a service by IPC using LISTSERV
1.8d To unsubscribe, send a message to [log in to unmask] with following
text in the BODY (NOT the subject field): SIGNOFF Leadfree To
temporarily stop/(start) delivery of Leadree for vacation breaks send:
SET Leadfree NOMAIL/(MAIL) Search previous postings at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
------------------------------------------------------------------------
-------
------------------------------------------------------------------------
-------Leadfee Mail List provided as a service by IPC using LISTSERV
1.8d To unsubscribe, send a message to [log in to unmask] with following
text in the BODY (NOT the subject field): SIGNOFF Leadfree To
temporarily stop/(start) delivery of Leadree for vacation breaks send:
SET Leadfree NOMAIL/(MAIL) Search previous postings at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
------------------------------------------------------------------------
-------
-------------------------------------------------------------------------------Leadfee Mail List provided as a service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Leadfree
To temporarily stop/(start) delivery of Leadree for vacation breaks send: SET Leadfree NOMAIL/(MAIL)
Search previous postings at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-------------------------------------------------------------------------------
|