For hole wall pull away I agree. Another factor is the topography of
the barrel. Smooth/polished resin areas readily have dep adhesion
failures and the larger the non-reinforced area the more pronounced.
Plasma etch processes can present issues with polishing the resin
interface and a post process to micro-roughen the resin areas is
important.
Jeffrey Bush
Director, Quality Assurance and Technical Support
VERMONT CIRCUITS INCORPORATED
76 Technology Drive - POB 1890
Brattleboro, Vermont 05302
Voice - 802.257.4571 ext 21
Fax - 802.257.0011
<http://www.vtcircuits.com/>
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Paul Reid
Sent: Thursday, August 03, 2006 5:32 PM
To: [log in to unmask]
Subject: Re: [TN] Barrel to Laminate Adhesion loss
Significant out gassing from volatiles gernerated during heating, can
contribute to separating the plated barrel from the drilled hole wall.
During lead-free thermal excursions, there is a greater propensity for
out gassing. Some materials are on the cusp of a chemical breakdown at
260C. Some of the delamination we have seen presents as bubbles in the
dielectric suggesting the dielectric system has failed and gasses are
being generated. Other materials, however, show a dappled, mottled
look, a condition that may be a precursor to gross material breakdown,
and exhibit hole wall pull away.
We have seen hole wall pull away pull the internal pad into the hole.
The internal pad can be displaced inward instead of breaking at the
interconnection. We call that condition "pad pull away". Three point
contact would increase robustness of the intenal interconnection and the
propensity for pad pull away over post separation. I expect that
misregistration of the drilled hole to the internal pad would aggrivate
"pad pull away".
My visceral reaction is that out gasing may be capable of producing
greater intra-barrel pressures than the stress exerted by X/Y axis
expansion, resin shrinage and CTE mismatches.
Paul Reid
Program Coordinator
PWB Interconnect Solutions Inc.
235 Stafford Rd., West, Unit 103
Nepean, Ontario
Canada, K2H 9C1
613 596 4244 ext. 229
[log in to unmask] <mailto:[log in to unmask]>
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Jeffrey Bush
Sent: Thursday, August 03, 2006 2:39 PM
To: [log in to unmask]
Subject: Re: [TN] Barrel to Laminate Adhesion loss
You will see less post separation with a 3 point connection as the post
if held in place during thermal expansion. The propensity for stresses
to the post connection are related to the expansion coefficient of the
package in the x, y and z axis. The CTE mismatch of the copper, glass
and resin are major contributors to the stresses introduced to the
package components during thermal cycling. The resins system will also
shrink as the degree of cure is advanced slightly during thermal
excursion, which propagates lateral stresses to the post connections as
the pad is pulled from the barrel. The z axis expansion contributes to
the separation by weakening the attachment. Excessive resin recession
can be an indication of an under-cured package as the advancement of the
cure increases.
Jeffrey Bush
Director, Quality Assurance and Technical Support
VERMONT CIRCUITS INCORPORATED
76 Technology Drive - POB 1890
Brattleboro, Vermont 05302
Voice - 802.257.4571 ext 21
Fax - 802.257.0011
<http://www.vtcircuits.com/>
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Rodney Miller
Sent: Thursday, August 03, 2006 11:09 AM
To: [log in to unmask]
Subject: Re: [TN] Barrel to Laminate Adhesion loss
So Anchoring barrel wall is not recommended on higher Tg/Td laminate
systems due to Cu CTE...
Could I get a copy of that White paper? I'm interested in the cause
effect also...
We have seen similare problems arise from trace/pad interface and
fracturing. If what you say is good for Barrel, this may also have
limits that are being exceeded. Our conventional wisdom is to teardrop
or filet the interface from Annular ring to Trace, to help with the
migration of a mechanical fracture.
Will this logic still apply?
LoHst and Confused...
-----Original Message-----
From: Werner Engelmaier [mailto:[log in to unmask]]
Sent: Wednesday, August 02, 2006 5:23 PM
Subject: Re: Barrel to Laminate Adhesion loss
Hi Richard & All,
Actually, the higher occurrances of hole wall separation and trace
separation
are not so much caused by more lateral stresses, but the different
thermal
and mechanical properties of SAC solders.
To understand what is happening, one really needs to understand what the
whole damage process causing hole wall separation [sometimes also called
resin
recession] and inner-layer separation [also called post separation or
trace
separation.
(1) On heating the resin expands-because of the glass fiber
reinforcement it
is prevented to expand in x/y and thus expands in z at nearly 3-times
its
thermal expansion without the glass reinforcement]; there is an
exception to this- the resin also tries to expand into the volume
occupied by the PTH, and is of
course, to some degree at least, prevented from doing so by the Cu
barrel
plating.
Thin Cu plating and/or large separation between inner-layer land
[serving as
anchors] encourage larger bulging inwards of the Cu with plastic
deformation
of the Cu.
(2) On cooling, the resin contracts to its former volume-if the Cu is
plastically deformed to a significant degree, it cannot do so: the
result=>hole wall
separation, and near the surface in connection with land rotation
inner-layer
separation.
(3) For SnPb solders the Solidus is 183C; thus, Solidus - Tg
(183-170C)~13C. For SAC solders the solidus is 217C; thus, Solidus - Tg
(217-170C)~47C. The consequence is that the delta-T after solder
solidification is about
4-times larger for SAC-solders, over which the high above Tg-thermal
contraction
acts-and this also holds the Cu back to its former position: the result
=>more
hole wall separation, and inner-layer separation.
Pretty straight-forward when you think about.
Werner
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|