TECHNET Archives

August 2006

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Thu, 3 Aug 2006 08:19:50 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Stadem, Richard D." <[log in to unmask]>
Subject:
From:
"Stadem, Richard D." <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (64 lines)
Thank you for this excellent summary, Werner. You have educated us all. 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier
Sent: Wednesday, August 02, 2006 5:23 PM
To: [log in to unmask]
Subject: Re: [TN] Barrel to Laminate Adhesion loss

Hi Richard & All,
Actually, the higher occurrances of hole wall separation and trace
separation are not so much caused by more lateral stresses, but the
different thermal and mechanical properties of SAC solders.
To understand what is happening, one really needs to understand what the
whole damage process causing hole wall separation [sometimes also called
resin recession] and inner-layer separation [also called post separation
or trace separation.
(1) On heating the resin expands-because of the glass fiber
reinforcement it is prevented to expand in x/y and thus expands in z at
nearly 3-times its thermal expansion without the glass reinforcement];
there is an exception to this- the resin also tries to expand into the
volume occupied by the PTH, and is of course, to some degree at least,
prevented from doing so by the Cu barrel plating. 
Thin Cu plating and/or large separation between inner-layer land
[serving as anchors] encourage larger bulging inwards of the Cu with
plastic deformation of the Cu.
(2) On cooling, the resin contracts to its former volume-if the Cu is
plastically deformed to a significant degree, it cannot do so: the
result=>hole wall separation, and near the surface in connection with
land rotation inner-layer separation.
(3) For SnPb solders the Solidus is 183C; thus, Solidus - Tg
(183-170C)~13C.
For SAC solders the solidus is 217C; thus, Solidus - Tg (217-170C)~47C.
The consequence is that the delta-T after solder solidification is about
4-times larger for SAC-solders, over which the high above Tg-thermal
contraction acts-and this also holds the Cu back to its former position:
the result =>more hole wall separation, and inner-layer separation.

Pretty straight-forward when you think about.

Werner

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2