TECHNET Archives

July 2006

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Jose Marroquin <[log in to unmask]>
Date:
Wed, 5 Jul 2006 13:54:34 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Steve Gregory <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="us-ascii"
From:
Steve Gregory <[log in to unmask]>
Parts/Attachments:
text/plain (105 lines)
Well, this is a first. I won't say it's completely un-heard of because I
used to work for a company that shall remain nameless that used Cascade
dishwashing detergent in a dishwasher to clean assemblies...hey,
whatever works.

Let's take a look at Mr. Clean multipurpose cleaner. From the MSDS:

Chemical                                                CAS No / Unique
ID              Percent 
Fragrance(s)/perfume(s)                         000000-00-1  
Surfactant(s) (unspecified)                     000000-00-4  
Water                                           007732-18-5  
Isopropylamine dodecylbenzenesulfonate  026264-05-1  
C9-11 Pareth-3                                  068439-46-3
0.1-1.0 
Colorant/Pigment/Dye(s)                         999999-49-3  
Quality control agent(s)                        999999-49-8

Three of the ingrediants are surfactants. The Isopropylamine
Dodecylbenzenesulfonate is sometimes known as a anionic surfactant, and
the  C9-11 Pareth-3 is also sometimes known as a nonionic surfactant. I
don't know what the quality control agent is, and the colorant and
fragrance is pretty self explaining. So Mr. Clean is a fancy detergent. 

Personally, I would think if you are rinsing really, really well with DI
water, I wouldn't see a problem using it. There ARE other things that
are DESIGNED specifically for cleaning printed circuit assemblies, so
why not use them?

-Steve Gregory- 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Jose Marroquin
Sent: Wednesday, July 05, 2006 12:37 PM
To: [log in to unmask]
Subject: Re: [TN] Rocha Laminate Voids..

All,

Recently we clean up residue on some boards with multipurpose Mr. Clean.

Should I expect problems from it?

Thanks.


-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Susan Mansilla
Sent: Wednesday, January 04, 2006 5:16 PM
To: [log in to unmask]
Subject: Re: [TN] Rocha Laminate Voids..

If they are in the prepreg and are present as pressed, then there is a
mismatch between the prepreg and pressing conditions.  Are you able to
do a flow test on some sheets of prepreg alone to see if the % flow is
as  expected?
Can
you determine if you are getting the predicted thickness of  the prepreg
layer?  Are you able to determine if you are hitting the  correct temp
before you hit the higher pressure during the lamination  cycle?

Is the excess around the edges of the panel "frothy" in appearance?

Just little thoughts that I would use to attack and "fix" the  problem.

Susan

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2