This is great stuff. What are the ratios/concentration of the B-I
solution. Is the part saturate with B.I solution at ambient, vacuum
and/or pressure to force the solution into the crack, cavity.
Victor,
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Guenter Grossmann
Sent: Tuesday, June 06, 2006 6:00 AM
To: [log in to unmask]
Subject: Re: [TN] Antw: [TN] Finding cracked capacitors
Victor
Sure.
The solution absorbs X- ray and penetrates readily in small cracks.
However, it also penetrates underneath the component. This means that
after applying the solution the entire capacitor looks pretty dark. We
use the effect that the liquid evaporates easier from underneath the
component than in the crack (does not work with hand soldered devices
since in this case everything is blocked with flux residues and no B-I
solution can penetrate into the crack). With other words, we apply the
solution, start looking at the specimen as fast as possible and watch
how the picture is getting brighter. Usually the solution in the crack
stains the x- ray picture some seconds longer than the one underneath
the components. Quite tricky and often we have to repeat the procedure
to become confident about the results. And as I said we are not always
successful. Mostly the 3 methods are used one after the other to get the
puzzle together.
Best regards
Guenter
EMPA
Swiss Federal Laboratories for Materials Testing and Research Centre
for Reliability Guenter Grossmann, Senior Engineer
8600 Duebendorf
Switzerland
Phone: xx41 1 823 4279
Fax : xx41 1 823 4054
mail: [log in to unmask]
>>> [log in to unmask] 06.06.2006 12:44:58 >>>
Can you elaborate some more on item 3 with the Boron-Iodine solved in
methylene.....
Victor,
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Guenter Grossmann
Sent: Tuesday, June 06, 2006 2:42 AM
To: [log in to unmask]
Subject: [TN] Antw: [TN] Finding cracked capacitors
Ioan
We use 3 technologies to search cracks in ceramic caps:
1. Ultrasonic microscopy. Works pretty well if the cracks are not too
close to the termination and if the structure of the caps is not too
inhomogeneous. Otherwise you don't have a flat surface to couple the US
into the component or the signal noise ratio ist too bad.
2. Infrared microscopy. Only applicable if you have a connecting path
in the crack where you can pump some power though. I already thought
once that using a penetrating material with a certain conductivity could
help in this measurement but I didn't have the time to look at that in
depth.
3. X- Ray. Works with a penetrating liquid that absorbs X-Rays(Boron-
Iodine solved in methylene). However, you need to work with 100kV and a
detector with a good energy resolution and whenever possible 12bit
graphics since the ceramic of the caps is already absorbing a lot of the
X- rays. Plus some tricks in handling.
And its still not sure that we find the bastards.
Best regards
Guenter
EMPA
Swiss Federal Laboratories for Materials Testing and Research Centre
for Reliability Guenter Grossmann, Senior Engineer
8600 Duebendorf
Switzerland
Phone: xx41 1 823 4279
Fax : xx41 1 823 4054
mail: [log in to unmask]
>>> [log in to unmask] 05.06.2006 16:11:04 >>>
Hi Technos,
a never ending story, ceramic caps that crack, possibly due to
depanelizing. The damage is not visible, unless the cap is cross
sectioned.
Is there any testing, thermal cycling or something like that, that could
show the damage real fast?
Thanks,
Ioan
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|