Gary
Tell engineering that a conformal coating does not SEAL against
moisture. All coatings breathe allowing air, that may contain
moisture, to move in and out of the coating film; and water, given
enough time, will go through everything...
Also inform them that thicker is not always better.
Acrylic coatings (Type AR) that are qualified to MIL-I-46058C and
meet IPC-CC-830 will perform optimally at a coating thickness of
0.002 ± 0.001 mils. (50 Micron ± 25 Micron).
The application you describe is not dissimilar to aircraft seat
entertainment systems - many using AR coatings - and you really don;t
want to know what people do in their aircraft seat! How about
superloos? These are street toilets that are fully automatic....use
your own imagination....and they use AR coatings.
I should be interested to understand your engineers proposed test
protocol...
Kindest regards
Graham Naisbitt
[log in to unmask]
Phone: +44 (0)12 5252 1500
Mobile: +44 (0) 79 6858 2121
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
Unit B2, Armstrong Mall
Southwood Business Park
Farnborough Hampshire
GU14 0NR - UK
ENGINEERING RELIABILITY
IN ELECTRONICS
DISCLAIMER : This message is intended only for the use of the
individual or entity to which it is addressed and may contain
information which is privileged, confidential, proprietary, or exempt
from disclosure under applicable law. If you are not the intended
recipient or the person responsible for delivering the message to the
intended recipient, you are strictly prohibited from disclosing,
distributing, copying, or in any way using this message. If you have
received this communication in error, please notify the sender and
destroy and delete any copies you may have received. Any views or
opinions presented in this email are solely those of the author and
might not represent those of Gen3 Systems Limited. Although Gen3
Systems Limited has taken reasonable precautions to ensure no viruses
present in this email, Gen3 Systems Limited can not accept the
responsibility for any loss or damage arising from the use of this
email or attachments.
On 20 Jun 2006, at 16:35, Bremer, Gary wrote:
> Engineering is recommending that we increase the thickness of the
> AR coating to .005 ± .002 to seal the boards against moisture.
> These boards are used on Boeing aircraft, my thought is to use UR
> coating due to the environment these boards are used.
>
>
>
> Is the Acrylic conformal coating the best choice for this application?
>
>
>
> Are there any problems with increasing the thickness of the Acrylic
> conformal coating?
>
>
>
> This box is open to the environment and with my knowledge of the
> mounting location the sanitary lines could be located above the
> electronics.
>
>
>
> Thanks
>
> Gary Bremer
> Senior Manufacturing Engineer, CIT
>
> Curtiss-Wright Controls Inc.
> Embedded Computing -Subsystem
>
> 28965 Avenue Penn
> Santa Clarita, CA 91355-4185
> Main: 661.257.4430 extension 2170
> Fax: 661.257.4782
>
>
> e-mail: [log in to unmask] <mailto:[log in to unmask]>
> Web: www.cwcembedded.com <http://www.cwcembedded.com>
>
> NOTICE: This e-mail communication is private and confidential and
> is intended for the addressee only. The email may only be used for
> conducting business with VISTA Controls Inc., dba Curtiss-Wright
> Controls Embedded Computing Subsystems. If you are not the intended
> recipient, please notify us by replying to this email followed by
> deleting the email and all attachments from your system. Anyone
> other than the intended recipient or those with a need to know
> within the recipient's organization is strictly prohibited from
> using, printing, distributing or disseminating the email or any
> information or attachment contained therein.
>
>
>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following
> text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail
> to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/
> archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?
> Pageid=4.3.16 for additional information, or contact Keach Sasamori
> at [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|