TECHNET Archives

June 2006

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Stadem, Richard D." <[log in to unmask]>
Date:
Thu, 22 Jun 2006 11:16:46 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Jeffrey Bush <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="us-ascii"
From:
Jeffrey Bush <[log in to unmask]>
Parts/Attachments:
text/plain (124 lines)
This is a very good point.  A woven/directional reinforcement certainly
gives a continuous opportunity for CAF formation sites, but in reality
the distance of the formation path is small and due to close proximity
of isolated utilities.  Non-directional/chopped/matted/etc. reinforments
are still present more than sufficient lengths to accommodate CAF
formations.  

Jeffrey Bush
Director, Quality Assurance and Technical Support
VERMONT CIRCUITS INCORPORATED 
           76 Technology Drive - POB 1890 
              Brattleboro, Vermont 05302
                Voice - 802.257.4571 ext 21
                    Fax - 802.257.0011
                       <http://www.vtcircuits.com/> 
                           

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.
Sent: Thursday, June 22, 2006 9:06 AM
To: [log in to unmask]
Subject: Re: [TN] Board material

In about 1978, when CAF was realized as a problem in standard PTH power
supply boards, the strands were continuous through the pre-preg. It was
then that the fab shops started to used chopped fiberglass mat weave, in
order to provide shorter strand lengths so CAF formation was less likely
to happen. However, because of circuitry being so close together
sometimes with fairly high potential, CAF has become more of an issue
again. 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Dehoyos, Ramon
Sent: Thursday, June 22, 2006 7:36 AM
To: [log in to unmask]
Subject: Re: [TN] Board material

        Hi Werner, could you expand on "Having PCB materials without
continuous glass fibers makes them immune to internal CAFs"?  I was
under the impression that the continuous glass fibers were the strength
of the board.
        Regards,	
        Ramon

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier
Sent: Wednesday, June 21, 2006 3:58 PM
To: [log in to unmask]
Subject: Re: [TN] Board material

Hi George,
CAF stands for 'Conductive Anodic Filament'-CAFs are capillary paths,
typically from PTH to PTH, along the glass fibers of the PCB glass fiber
reinforcements. The get started by damage done during PTH drilling with
a dull drill, propagate further depending on internal vapor pressures,
and on application of a potential difference transport metallic ions
forming a conductive path. Now, this conductive path does not give you a
dead open, but lowers insulation resistance by couple of orders of
magnitude. 
Having PCB materials without continuous glass fibers makes tham imune to
internal CAFs.

Regards,
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Cell: 386-316-5904
E-mail: [log in to unmask], Website: www.engelmaier.com

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2