TECHNET Archives

June 2006

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Adam Seychell <[log in to unmask]>
Date:
Tue, 13 Jun 2006 06:11:28 -0700
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, R Sedlak <[log in to unmask]>
Subject:
From:
R Sedlak <[log in to unmask]>
Content-Transfer-Encoding:
8bit
In-Reply-To:
Content-Type:
text/plain; charset=iso-8859-1
MIME-Version:
1.0
Parts/Attachments:
text/plain (64 lines)
Adam:  I am impressed, for a guy who claims his chemistry is not that good, you are doing a better job than most...
  Yes, you can use the ORP reading in an ammoniacal etcher as well as Cupric, and this would be a great way to monitor Cuprous.   You can also do a titration with Iodine, but I have a sense that getting the sample, neutralizing and diluting it would probably allow most of the Cuprous to be converted to Cupric, so your titration would probably be meaningless.

  For a review of this chemistry, and I am not sure you need it, you may want to check out our website, www.pcbfab.com

  Rudy Sedlak

Adam Seychell <[log in to unmask]> wrote:
  I am wondering if there is a simple test for cuprous ions in ammoniacal
chloride alkaline etching, and thus determine when to increases or
decrease the air ventilation intake of the etching machine. I am brewing
my own chemistry based on typical operating parameters of ammoniacal
chloride etchants.

Copper 2 ~ 2.5 Molar
Chloride 4.5 ~ 5 Molar
pH 8.0 ~ 8.6
Temp. 40 ~ 45 °C

I discovered just like with acid cupric chloride etching, that when the
cuprous content reaches to even small concentrations then the etch rate
is severely affected. In the lab, I tested as little as 5g/L of
dissolved copper in the cuprous state will slow etch rate, and at 10 g/L
it becomes virtually a stand still. For acid copper chloride etchants,
the loss of its bright green color is a quick indicator of cuprous ions
being present, and even 0.5 g/L will show beginnings of color change.
However in alkaline etching the cuprous ions do not appear visible or
change the solution color. I have heard about ORP (oxidation-reduction
potential) probes used in acid cupric chloride machines. Can these same
probes be used in ammoniacal chloride etchants ?

My chemistry is a bit poor, although I'm wondering if is possible to
make such a probe, using a standard reference electrode (e.g Ag/AgCl )
and a piece of copper wire as the indicator electrode.


Adam Seychell

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------


 __________________________________________________
Do You Yahoo!?
Tired of spam?  Yahoo! Mail has the best spam protection around

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
http://mail.yahoo.com

ATOM RSS1 RSS2