As a clarification, immersion tin chemistries that contain high amounts of
organics claim reduced whisker risk. For electrolytically deposited tin,
organics are typically greatly reduced in modern tin plating chemistries
that target whisker mitigation. The electrolytic bright tins have
historically contained more organics and have been more closely related to
whisker problems than the matte tins that contain much lower organics.
These electrolytic tins are always used on the leadframes of IC components,
unless an alternative PbFree lead finish is used.
Best regards,
Leo
Leo M. Higgins III, Ph.D.
Vice President, Technical Operations
ASAT, Inc.
3755 Capital of Texas Highway, Suite 100
Austin, Texas 78704
office phone 512-383-4593
mobile 512-423-2002
[log in to unmask]
www.asat.com
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Kane, Amol (349)
Sent: Wednesday, June 21, 2006 10:31 AM
To: [log in to unmask]
Subject: Re: [TN] Blowholes pandemic
One reason the organics would be in Sn plating is to mitigate the risk of
Tin whiskers, another reason is to prevent tarnishing of the surface finish
Amol Kane
M.S (Industrial Eng.)
Process Engineer
Harvard Custom Manufacturing
941 Route 38 Owego, NY 13827
Phone: (607) 687-7669 x349
[log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Tempea, Ioan
Sent: Wednesday, June 21, 2006 11:26 AM
To: [log in to unmask]
Subject: Re: [TN] Blowholes pandemic
Thanks Mike and Rudy!
I will change my question to: what on Earth are the organics doing in the
plating? Is this normal?
Any suggestions on how to control the AVL or the Incoming inspection of
these parts to avoid the issue?
Thanks,
Ioan
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of R Sedlak
Sent: Wednesday, June 21, 2006 11:12 AM
To: [log in to unmask]
Subject: Re: [TN] Blowholes pandemic
I will go farther, and suggest that Mike is almost certainly correct, this
being the source of most "blowholes".
Rudy Sedlak
"Barmuta, Mike" <[log in to unmask]> wrote: Ioan: The blowholes you are
seeing could be the result of organics in
the tin plating outgassing during reflow. When heated they release CO
and CO2 gases creating voids.
Regards
Michael Barmuta
Staff Engineer
Fluke Corp.
Everett WA
425-446-6076
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Tempea, Ioan
Sent: Wednesday, June 21, 2006 5:57 AM
To: [log in to unmask]
Subject: [TN] Blowholes pandemic
Hi Technos,
for a couple of days I see occurences of blowholes in the joints of,
guess what, SMT 0603 resistors.
The reflow recipe did not change and we're talking about 2 different
established products, we have run many of each before. One is WS, the
other one no-clean. Each one uses different brand of solder paste, SnPb.
I have changed the paste with fresh one, no positive results. I have
changed the reels with different date codes, Bingo! But even the "bad"
parts were quite fresh, less than one year old. One of them is pure Sn
plated, don't know about the other ones.
The question is: where on Earth can humidity stay in a ceramic resistor?
What else can be the cause of the blowholes? Did not bake the boards,
since changing the components worked, so I guess the PCBs are out of the
hook...
Thanks,
Ioan
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
This message (including any attachments) contains confidential
and/or proprietary information intended only for the addressee.
Any unauthorized disclosure, copying, distribution or reliance on
the contents of this information is strictly prohibited and may
constitute a violation of law. If you are not the intended
recipient, please notify the sender immediately by responding to
this e-mail, and delete the message from your system. If you
have any questions about this e-mail please notify the sender
immediately.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------
Do you Yahoo!?
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
Get on board. You're invited to try the new Yahoo! Mail Beta.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
CONFIDENTIALITY NOTICE:
This e-mail, and any attachments, is for the sole use of the intended
recipient(s) and may contain information that is confidential and
protected from disclosure under the law. Any unauthorized review, use,
disclosure, or distribution is prohibited. If you are not the intended
recipient, please contact the sender by reply e-mail, and delete/destroy
all copies of the original message and attachments.
Thank you.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|