Looks like what could be nailing you is the 71C Tg with the moderately
high (as far as conformal coats go) Young's modulus of about 13,000psi.
Spray applying is a good solution. It would be good to go through the
calculations of how much stress you're applying to the glass seal from
the cure condition to the -51C where its getting fractured, and verify
that the glass seals are as strong as they're supposed to be. That way
you can have more confidence in the engineering fix.
Wayne
>>> [log in to unmask] 5/22/2006 1:17 pm >>>
Hello, again...
All indications are leading to the conformal coating as the culprit for
the
cracked 8-pin DIPs. The urethane coating (Humiseal 1A20) is
dip-applied,
and a typical assembly has bridging between the component body and the
PWB,
as well as between the component body and the leads. Ten ESS thermal
cycles
of -51 to +85C prior to coating showed no cracks, but samples cycled
after
coating had some cracks. My suggestion to the supplier was to
spray-apply
the coating and inspecting for coating bridging.
Have you experienced anything like this before?
Jim Marsico
Senior Engineer
Production Engineering
EDO Corporation
[log in to unmask] <mailto:[log in to unmask]>
631-630-5079
-----Original Message-----
From: Russ Winslow [SMTP:[log in to unmask]]
Sent: Wednesday, May 10, 2006 5:58 PM
To: TechNet E-Mail Forum; Marsico, James
Subject: RE: [TN] Cracked ICs
Hello James,
Here are a few things to look for. The 8-pin cerdip package
does
not have much surface area for the glass seal especially if the die is
large. A lead forming step prior to board assembly could be the cause.
If
you are forming the leads inward be certain that only the minor leads
(the
skinny portion) are being bent. If the major leads (the wide portions)
are
bent simultaneously then you may very well pop the cap from the base
or
cause these perimeter cracks. Another thing to look for is cracks
before
board assembly. Cerdips are prone to glass cracking caused by tube to
tube
handling. I have never heard of cracking due to reflow process unless
you
are doing vapor phase without preheat. Some automatic lead
straighteners
will crack 1000 units per hour so do not let them come anywhere near
your
glass sealed components. Another cause could be a lead tinning (hot
solder
dip) step. Without proper preheat a supplier could cause serious
damage to
the glass seal.
If you send me a sample I can probably tell you much more. (no
charge!)
Regards,
Russ Winslow
Six Sigma
905 Montague Expwy
Milpitas, CA 95035
[log in to unmask]
www.sixsigmaservices.com
Phone (408) 956-0100 x 111
Fax (408) 956-0199
-----Original Message-----
From: Marsico, James [mailto:[log in to unmask]]
Sent: Wednesday, May 10, 2006 6:11 AM
To: [log in to unmask]
Subject: [TN] Cracked ICs
Hello Technet,
We're seeing a recurring problem of a cracked ceramic IC,
assembled
on a
through-hole PWB. The component is an 8-pin DIP, T.I. P/N
5962-9452601QPA .
The crack is located below the lead frame and radiates all the
way
around
the device. Has anyone experienced this before?
Please respond directly to me, as I cannot receive e-mails
from
Technet.
Thanks in advance,
Jim Marsico
Senior Engineer
Production Engineering
EDO Corporation
[log in to unmask] <mailto:[log in to unmask]>
631-630-5079
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV
1.8e
To unsubscribe, send a message to [log in to unmask] with
following
text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send
e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail
to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information,
or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|