Genny: Good point. I think the problem may be when soldering with
leadfree solder directly to brass containing 4%Pb does the amount of Pb
dissolved in the solderjoint exceed the 0.1% BW limit of RoHS.
Regards
Mike B.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Genny Gibbard
Sent: Tuesday, March 21, 2006 10:01 AM
To: [log in to unmask]
Subject: Re: [TN] PB-Free Solder and Brass
Would brass fall under exemption #6 from the directive annex?
Lead as an alloying element in steel containing up to 0,35 % lead by
weight, aluminium containing up to 0,4 % lead by weight and as a copper
alloy containing up to 4 % lead by weight.
Which may mean the brass can contain Pb and still be "compliant", but
solder used for soldering to it cannot. That might explain the need for
Pbfree solder - to maintain RoHS compliance.
However, I'm not a metallurgist, so ...
Genny.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: March 21, 2006 11:12 AM
To: [log in to unmask]
Subject: Re: [TN] PB-Free Solder and Brass
Hi Mark! One additional comment to add to Mike's information. Brass is
an alloy of copper and zinc. One potential problem when soldering to a
brass alloy is the zinc content causing long term solder joint integrity
issues.
De-zincification is where the zinc preferentially diffuses into the
solder joint potentially causing solder joint failures. The way to avoid
this phenomena is to plate the brass with a barrier layer such as copper
or nickel. You might check to see if the contacts have a barrier layer.
Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
"Barmuta, Mike"
<Mike.Barmuta@FLU
KE.COM>
To
Sent by: TechNet [log in to unmask]
<[log in to unmask]>
cc
Subject
03/21/2006 09:51 Re: [TN] PB-Free Solder and Brass
AM
Please respond to
TechNet E-Mail
Forum
<[log in to unmask]>
; Please respond
to
"Barmuta, Mike"
<Mike.Barmuta@FLU
KE.COM>
Hi Mark: First of all it doesn't make sense why the customer wants to
use a leadfree solder on a leaded (C360 brass) component. It won't be
RoHS compliant. What is there reason for asking for leadfree solder?
However if ours is not to question why then give them what they are
asking for; leadfree solder.
You may have oxidized parts and need a stronger flux/deoxidizer. As a
test try dipping a few in 5% sulfuric acid for 20-30 seconds at room
temp, rinse well with cold water and dry immediately.
See if they wet better. If they do then use the acid predip or a
stronger fluxing agent. If they don't you could always tin plate them
along with a copper or nickel barrier plate and solder to the tin.
Regards
Michael Barmuta
Staff Engineer
Fluke Corp.
Everett WA
425-446-6076
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Mark Clark
Sent: Tuesday, March 21, 2006 6:52 AM
To: [log in to unmask]
Subject: [TN] PB-Free Solder and Brass
I have a customer that is required to use a Lead Free solder to attach
some brass components (battery contacts) to a PCB. What he is
experiencing is the brass will not tin using this solder. Anyone have
any suggestions:
Solder required for use:
Cookson Electronics - Alpha Cleanline 7000
Alloy 96.5Sn 3.0Ag 0.5Cu
Flux: P2
The contact material is:
360Brass
His customer is in a rush for these components, and is demanding the
Pb-free be used.
BTW - the good old fashion No-clean and Rosin (both of these have lead
in
them) work great.
TIA
Mark Clark
Avalon Engineering, LLC
2179 Fourth Street, Suite 2D
PO Box 10789
White Bear Lake, MN 55110-0789
Phone: 651-426-8599 x202
Fax: 651-426-4418
mailto:[log in to unmask]
www.avalon-us.com
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
This message (including any attachments) contains confidential
and/or proprietary information intended only for the addressee.
Any unauthorized disclosure, copying, distribution or reliance on
the contents of this information is strictly prohibited and may
constitute a violation of law. If you are not the intended
recipient, please notify the sender immediately by responding to
this e-mail, and delete the message from your system. If you
have any questions about this e-mail please notify the sender
immediately.
Ce message (ainsi que les eventuelles pieces jointes) est
exclusivement adresse au destinataire et contient des
informations confidentielles. La copie, la communication ou la
distribution du contenu de ce message sans l'accord prealable de
l'expediteur sont strictement interdits et peuvent constituer un
delit. Si vous n'etes pas destinataire de ce message, merci de le
detruire et d'avertir l'expediteur. Si vous avez des questions se
rapportant a ce courrier electronique, merci de bien vouloir
notifier
l'expediteur immediatement.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|