In general bright tin finishes, which contain high levels of grain refiners
and have very fine grain sizes, show much greater incidence of whiskering
than matte tin finishes (99+ % Sn) with very low amounts of grain refiners
and a coarser microstructure. With leaded IC packages a Ni underplate has
been shown to provide some benefit in whisker reduction, but matte tin over
Ni over a copper leadframe cannot be claimed to provide a guaranteed
whisker-free package. So, I think a Ni underplate would be much less likely
to reduce whiskering with a bright tin finish than it would be with a matte
tin finish. This is based upon work with leaded IC packages, but I suspect
much of this learning is applicable to a like board finish.
Best regards,
Leo
Leo M. Higgins III, Ph.D.
Vice President, Technical Support Operations
ASAT, Inc.
3755 Capital of Texas Highway, Suite 100
Austin, Texas 78704
office phone 512-383-4593
mobile 512-423-2002
[log in to unmask]
www.asat.com
The information contained in this electronic message is CUSTOMER/SUPPLIER
PRIVILEGED AND CONFIDENTIAL INFORMATION intended only for the use of the
individual or entity named above. If the reader of this message is not the
intended recipient, you are hereby notified that any dissemination,
distribution and copying of this communication is strictly prohibited. If
you have received this communication in error, please immediately notify the
sender by electronic mail. Thank you.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Stadem, Richard D.
Sent: Thursday, March 16, 2006 4:16 PM
To: [log in to unmask]
Subject: [TN] FW: [TN] Immersion Tin Specification
-----Original Message-----
From: Stadem, Richard D.
Sent: Thursday, March 16, 2006 4:12 PM
To: 'Vladimir Igoshev'
Subject: RE: [TN] Immersion Tin Specification
My apologies, Vladimer. I double checked my information. I have a finish
provider whose documentation for a bright tin finish on the PWB claims
it is "whisker-free". That confused me. I went back over the references
I have (NEMI report and "Tin Whiskers: Attributes and Mitigation" by J.
Brusse, G. Ewell and J. Siplon, and other references)and they support
what you are saying. The finish vendor apparently recommends putting the
bright tin over a nickel base, which supposedly mitigates the whisker
formation. Does this make sense?
There is so much conflicting information amongst those providing tin
finishes for components versus tin finishes for circuit boards it is
hard for me to keep it all straight.
-----Original Message-----
From: Vladimir Igoshev [mailto:[log in to unmask]]
Sent: Thursday, March 16, 2006 3:52 PM
To: Stadem, Richard D.
Subject: Re: [TN] Immersion Tin Specification
Richard,
Can you send me the referrence? Unless I'm completely confused, that is
not what I've been hearing.
Vladimir
Sent from my Blackberry Wireless
Vladimir Igoshev, 519-888-7465 ext.5283
----- Original Message -----
From: Stadem, Richard D. <[log in to unmask]>
To: Vladimir Igoshev
Sent: Thu Mar 16 16:47:42 2006
Subject: RE: [TN] Immersion Tin Specification
Thank you. Then why is it reported that matte tin has a greater tendency
to incur tin whiskers? Would it be because of a higher stress factor in
the grain?
-----Original Message-----
From: Vladimir Igoshev [mailto:[log in to unmask]]
Sent: Thursday, March 16, 2006 3:43 PM
To: [log in to unmask]; Stadem, Richard D.
Subject: Re: [TN] Immersion Tin Specification
As far as I know, immersion tin is better than mette and of cause bright
ones
Vladimir
Sent from my Blackberry Wireless
Vladimir Igoshev, 519-888-7465 ext.5283
----- Original Message -----
From: TechNet <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Thu Mar 16 16:39:34 2006
Subject: Re: [TN] Immersion Tin Specification
Better than what? Better than it used to be? Could you clarify, as I am
wondering what you mean by that. Thanks.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Vladimir Igoshev
Sent: Thursday, March 16, 2006 3:29 PM
To: [log in to unmask]
Subject: Re: [TN] Immersion Tin Specification
Ramon,
Immersion Tin is MUUUUUCH better in terms of whiskering.
Vladimir
Vladimir Igoshev, Ph. D.
Manager, Metallurgical Lab
Research in Motion
451 Phillip St.
Waterloo, ON, N2L 3X2
Voice: (+1) 519-888-7465, ext. 5283
Fax: (+1) 519-886-0863
E-mail: [log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Dehoyos, Ramon
Sent: Thursday, March 16, 2006 4:12 PM
To: [log in to unmask]
Subject: Re: [TN] Immersion Tin Specification
John:
Just curious, what is the tin plating going to be used
on? Thin Tin plating produces whiskers, which can be a nightmare.
Thicker Tin plating helps as a whisker mitigating factor. These whiskers
have shot down a nuclear power plant and caused space craft failures.
Tin plating can very problematic. Whiskers can grow in days or take
years.
Regards,
Ramon
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of R Sedlak
Sent: Thursday, March 16, 2006 4:01 PM
To: [log in to unmask]
Subject: Re: [TN] Immersion Tin Specification
John: Generally accepted goal is one micron, or 40 microinches,
thickness.
You essentially never have to worry about it being too thick, and
thickness of less than 75% of that value should raise eyebrows...
Rudy Sedlak
RD Chemical Company
John Parsons <[log in to unmask]> wrote: IPC have graciously
provided us (the industry) with specifications for ENIG
(IPC-4552) and Immersion Silver (IPC-4553), is there a similar
specification Immersion Tin (white tin)? If not, is there a generally
accepted specification for material thickness?
John Parsons
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------
Brings words and photos together (easily) with
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
PhotoMail - it's free and works with Yahoo! Mail.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential
information, privileged material (including material protected by the
solicitor-client or other applicable privileges), or constitute
non-public information. Any use of this information by anyone other than
the intended recipient is prohibited. If you have received this
transmission in error, please immediately reply to the sender and delete
this information from your system. Use, dissemination, distribution, or
reproduction of this transmission by unintended recipients is not
authorized and may be unlawful.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential
information, privileged material (including material protected by the
solicitor-client or other applicable privileges), or constitute
non-public information. Any use of this information by anyone other than
the intended recipient is prohibited. If you have received this
transmission in error, please immediately reply to the sender and delete
this information from your system. Use, dissemination, distribution, or
reproduction of this transmission by unintended recipients is not
authorized and may be unlawful.
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential
information, privileged material (including material protected by the
solicitor-client or other applicable privileges), or constitute
non-public information. Any use of this information by anyone other than
the intended recipient is prohibited. If you have received this
transmission in error, please immediately reply to the sender and delete
this information from your system. Use, dissemination, distribution, or
reproduction of this transmission by unintended recipients is not
authorized and may be unlawful.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|