Hi Mark! One additional comment to add to Mike's information. Brass is an
alloy of copper and zinc. One potential problem when soldering to a brass
alloy is the zinc content causing long term solder joint integrity issues.
De-zincification is where the zinc preferentially diffuses into the solder
joint potentially causing solder joint failures. The way to avoid this
phenomena is to plate the brass with a barrier layer such as copper or
nickel. You might check to see if the contacts have a barrier layer. Good
Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
"Barmuta, Mike"
<Mike.Barmuta@FLU
KE.COM> To
Sent by: TechNet [log in to unmask]
<[log in to unmask]> cc
Subject
03/21/2006 09:51 Re: [TN] PB-Free Solder and Brass
AM
Please respond to
TechNet E-Mail
Forum
<[log in to unmask]>
; Please respond
to
"Barmuta, Mike"
<Mike.Barmuta@FLU
KE.COM>
Hi Mark: First of all it doesn't make sense why the customer wants to
use a leadfree solder on a leaded (C360 brass) component. It won't be
RoHS compliant. What is there reason for asking for leadfree solder?
However if ours is not to question why then give them what they are
asking for; leadfree solder.
You may have oxidized parts and need a stronger flux/deoxidizer. As a
test try dipping a few in 5% sulfuric acid for 20-30 seconds at room
temp, rinse well with cold water and dry immediately.
See if they wet better. If they do then use the acid predip or a
stronger fluxing agent. If they don't you could always tin plate them
along with a copper or nickel barrier plate and solder to the tin.
Regards
Michael Barmuta
Staff Engineer
Fluke Corp.
Everett WA
425-446-6076
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Mark Clark
Sent: Tuesday, March 21, 2006 6:52 AM
To: [log in to unmask]
Subject: [TN] PB-Free Solder and Brass
I have a customer that is required to use a Lead Free solder to attach
some
brass components (battery contacts) to a PCB. What he is experiencing
is
the brass will not tin using this solder. Anyone have any suggestions:
Solder required for use:
Cookson Electronics - Alpha Cleanline 7000
Alloy 96.5Sn 3.0Ag 0.5Cu
Flux: P2
The contact material is:
360Brass
His customer is in a rush for these components, and is demanding the
Pb-free
be used.
BTW - the good old fashion No-clean and Rosin (both of these have lead
in
them) work great.
TIA
Mark Clark
Avalon Engineering, LLC
2179 Fourth Street, Suite 2D
PO Box 10789
White Bear Lake, MN 55110-0789
Phone: 651-426-8599 x202
Fax: 651-426-4418
mailto:[log in to unmask]
www.avalon-us.com
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|