Hi folks! Just an FYI. The use of stranded silver coated wire has the
potential of causing corrosion issues. As Rainer and Bogert both pointed
out, silver coated wire has been successfully used in high performance
electronics for many years without issues. However, there are documented
instances of specific use environments (e.g. direct marine exposure) where
using silver coated wire resulted in corrosion problems. Every material is
not suited for every use environment - the trick is to understand your use
environment and how protected/shielded your electronic product is from that
use environment.
Dave Hillman
Rockwell Collins
[log in to unmask]
March 11, 2006
We also have used stranded silver coated wire for years with no known
problem. Last year, I tried to convince the IPC folks responsible for IPC
7711/7721 to either delete their statement in the document not to use
silver coated wire, or otherwise provide the technical basis for the
statement. They did not provide any info and left the caution in the IPC
document.
I could not open the hyperlink address you gave in the e-mail. Can you
please e-mail me the article?
[log in to unmask]<mailto:[log in to unmask]>
I'm not sure what being lead-free has to do with corrosion, but here in
the Space Product business virtually all of our hard wiring and cabling
consists of silver plated copper wire. It's been that way for 40 years
and we have never seen or heard of any corrosion issue. We also use
solid wire with the same reliable results. The only corrosion that I
have ever heard of was called "Red Plague" in the early 1960's and was
the result of fractures in too thin silver plating. A galvanic reaction
was set up between copper and silver at the fracture line that slowly
consumed the copper. This was resolved by the wire industry by
increasing the thickness of silver plating. This corrosion is extremely
rare! Here is a link to a report on the subject.
http://nepp.nasa.gov/docuploads/97164203-A4FB-479A-A075C918D51DD81E/ESA%<
http://nepp.nasa.gov/docuploads/97164203-A4FB-479A-A075C918D51DD81E/ESA>
20Red%20Plague.pdf
> Rainer G. Blomberg
> Honeywell -Space Systems Clearwater
> Staff Production Engineer
(727) 539-5534
All:
We need to add a 30 AWG jumper wire to a lead-free assembly (Class
II). IPC-A-610 says that silver plated stranded wire should not be used
due to possible corrosion under certain conditions. Our thoughts are
that this (corrosion possibility) is unique to stranded wire. Would
silver plated solid wire be an alternative? Any input would be
appreciated. Thanks.
Regards,
Steve Vargas
Sr. Mfg. Engineer
Polaris Contract Mfg. Inc.
[log in to unmask]<mailto:[log in to unmask]>
508-748-3399 ext.192
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|