Chris,
Another tip:
I also had to qualify wave solder fluxes twice in the past two years for
a couple of clients. Both times I used many different fluxes to get
optimum hole fill and topside fillets, and both times Qualitek 775A beat
everybody. The Qualitek does require a robust cleaning system as it was
slightly more difficult to clean. But with a good machine wash system
there was no trouble. So as a result some operators tried using it as a
benchtop flux for hand soldering of difficult-to-solder high-mass
connectors similar to what you describe, and found that it helped
immensely. For the really difficult applications they soldered the
assembly right on a hot-plate set at 100 deg. C.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Schaefer, Chris
Sent: Tuesday, February 28, 2006 1:29 PM
To: [log in to unmask]
Subject: Re: [TN] Solder Joint Inspection
This is true. My point is that the customer may allow the 50% fill if
approached using some process data or other to support it. IPC rev. D ha
ha! we don't have that and won't for quite a while. Does rev. D say
anything different about this criteria? I know from a seminar I went to
a while back done by Keller in which depending on the end application
and environment - less solder is in fact better because it is not a
rigid joint.
Regards,
CAS
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Barmuta, Mike
Sent: Tuesday, February 28, 2006 1:22 PM
To: [log in to unmask]
Subject: Re: [TN] Solder Joint Inspection
Hi Chris: I think if you look closely at the wording in 6.3.1, 50 % hole
fill is not acceptable for class 3, only class 1 and 2.
Ken is building to class 3.
BTW You are probably looking at IPC-A-610 rev C. The new one is rev D
section 7.5.5.1
Regards
Michael Barmuta
Staff Engineer
Fluke Corp.
Everett WA
425-446-6076
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Schaefer, Chris
Sent: Tuesday, February 28, 2006 11:02 AM
To: [log in to unmask]
Subject: Re: [TN] Solder Joint Inspection
Section 6.3.1 speaks about a 50% vertical hole fill on sections of the
board that are considered thermal planes or conductor planes. It sounds
like this applies, but it may require something from your customer to
allow this or for reasons of stress it is required - not sure. We have
issues such as your and we have spoken with the customer and have
received the ok to allow a 50% fill versus the traditional 75%.
I agree with the previous point, but it will not allow for any process
anomalies that occur on occasion. If for some reason the connector has
issues related to the solderability, then you have a problem. In another
scenario if the area/ connector has not been proper fluxed or achieved
proper solder contact - it might look fine on the outside, but has not
achieved the solderability levels you desire.
Food for thought...
Have a nice day guys!
Chris Schaefer
Suntron Corporation
Process Engineer
540 N. Rogers Road
Olathe, Kansas 66062
913.393.5878
[log in to unmask]
NOTICE:
This message is intended for the use of the individual entity to which
it is addressed and may contain information that is privileged,
confidential and exempt from disclosure under applicable law. If the
reader of this message is not the intended recipient, or the employee or
agent responsible for delivering the message to the intended recipient,
you are hereby notified that any dissemination, distribution or copying
of this communication is strictly prohibited. If you have received this
communication in error, please notify us immediately by calling
913.393.5878 or returning the original message to us.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of John Berg
Sent: Tuesday, February 28, 2006 12:44 PM
To: [log in to unmask]
Subject: Re: [TN] Solder Joint Inspection
If x-ray is not an option, you need to set up a soldering process that
would not require inspection. On a thermally relieved pad that does not
get sufficient fill, you need to preheat the pad area prior to hand
soldering to compensate for the heat sinking. If you can get a dummy
populated board, preheat it to a known reference level, and then remove
the connector body to examine the % fill. Find the minimum reference
preheat that will obtain your desired % fill. If you can't get a dummy
populated board, you can use a few production boards to find the
reference preheat by utilizing an ouitside x-ray service to determine
the % fill.
>>> [log in to unmask] 2/28/2006 7:55 AM >>>
We are having a heck of a time inspecting some solder joints and could
use your help.
Per Class 3 a solder joint is supposed to have at least a 75% fill. We
have a circuit board that has large ground planes and hand soldered
connectors that are impossible to inspect for top side solder.
We do not have access to an x-ray and are wondering if there are any
clever ways to inspect these solder joints.
Thanks,
KennyB
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
This message (including any attachments) contains confidential and/or
proprietary information intended only for the addressee.
Any unauthorized disclosure, copying, distribution or reliance on the
contents of this information is strictly prohibited and may constitute a
violation of law. If you are not the intended recipient, please notify
the sender immediately by responding to this e-mail, and delete the
message from your system. If you have any questions about this e-mail
please notify the sender immediately.
Ce message (ainsi que les eventuelles pieces jointes) est exclusivement
adresse au destinataire et contient des informations confidentielles. La
copie, la communication ou la distribution du contenu de ce message sans
l'accord prealable de l'expediteur sont strictement interdits et peuvent
constituer un delit. Si vous n'etes pas destinataire de ce message,
merci de le detruire et d'avertir l'expediteur. Si vous avez des
questions se rapportant a ce courrier electronique, merci de bien
vouloir notifier l'expediteur immediatement.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|