Dissolution rate so slow it would take forever
Regards
Ian Fox
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Ivanoe Pedruzzi
Sent: 17 January 2006 09:13
To: [log in to unmask]
Subject: Re: [TN] enig bad board
Richard, I took from your email:
.....
With the flash gold over nickel or the ENIG plating the gold will be
absorbed into the solder and you will form a solder joint to the nickel.
....
The reason I asked about dissolution rate, temperature and time, is
that I assumed one could have the solder join formed with copper if the
Nickel is let completely to dissolve in the molten solder.
Do you think this is not feasible?
I value your opinion.
THX, Ivan
Il giorno 16/gen/06, alle ore 14:59, Stadem, Richard D. ha scritto:
> Others have responded that the cost of immersion silver is usually
> much less than ENIG.
> But what you need to consider also is whether to use the nickel with
> flash gold, standard electroless nickel/immersion gold (ENIG), or
> immersion silver.
> When soldering to the immersion silver finish the silver will be
> absorbed into the solder and the solder joint will be formed on
> copper.
> With the flash gold over nickel or the ENIG plating the gold will be
> absorbed into the solder and you will form a solder joint to the
> nickel.
> Either of the flash gold over nickel or ENIG requires plating of
> nickel, and as such the process is susceptible to nickel skips, which
> you have already experienced. Not much fun.
>
> The solder joints formed on copper will be stronger than those formed
> on nickel because of nickel's much slower rate of dissolution into the
> solder joint. Because of the slower dissolution rate, the assembly
> requires more heat, and for a longer time, especially under the BGAs.
> BGAs do an excellent job of insulating the solder spheres.
> If you have BGAs or chip scale components, you will be much better off
> with immersion silver finish on the PWB. If you have high impedance/
> high frequency circuitry you will also be much better off with
> immersion silver.
> Buy a sample of boards and qualify the assembly with the different
> plating no matter which one you choose.
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Sumxplore
> Sent: Friday, January 13, 2006 11:55 PM
> To: [log in to unmask]
> Subject: Re: [TN] enig bad board
>
> Looks like this is the beginning of my nightmare with more to come
> after reading those valuable feedback by technetters.
>
> No,I haven't try immersion silver but certainly I will explore
> it.Anyone can let me what is the cost differences between Immersion
> silver and ENIG?
>
> Thank you.
>
> ----- Original Message -----
> From: "Lee Parker" <[log in to unmask]>
> To: "'TechNet E-Mail Forum'" <[log in to unmask]>; "'sumxp'"
> <[log in to unmask]>
> Sent: Saturday, January 14, 2006 1:34 AM
> Subject: RE: [TN] enig bad board
>
>
>> Sumxp
>>
>> It is likely the thickness of the gold is inadequate and the
>> underlying nickel has oxidized. I would measure the gold thickness
>> (XRF) and compare it to the minimum specified. The silver color after
>> erasing is most likely the nickel that is under the gold and with the
> oxides removed.
>>
>> There are many other alternatives these days to ENIG such as
>> immersion
>
>> silver. Have you evaluated into any of these?
>>
>> Best regards
>>
>> Lee
>>
>> J. L. Parker Ph.D.
>> JLP Consultants LLC
>> (804) 779 3389
>>
>>
>> Best regards
>>
>> Lee
>>
>> J. L. Parker Ph.D.
>> JLP Consultants LLC
>> (804) 779 3389
>>
>>
>> -----Original Message-----
>> From: TechNet [mailto:[log in to unmask]] On Behalf Of sumxp
>> Sent: Friday, January 13, 2006 10:48 AM
>> To: [log in to unmask]
>> Subject: [TN] enig bad board
>>
>> Hi,
>>
>> We noticed few ENIG bga pads black in color instead of gold.It turn
>> silver when use eraser to remove away the black color pad.What is the
>> defect mode?
>> Any reliability issue?Is it advisable to continue using these pcbs?
>>
>> Thanks......
>>
>> ---------------------------------------------------
>> Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
>> unsubscribe, send a message to [log in to unmask] with following text
>> in
>
>> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
>> or (re-start) delivery of Technet send e-mail to
>> [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
>> per day of all the posts: send e-mail to
>> [log in to unmask]: SET Technet Digest
>> Search the archives of previous posts at:
>> http://listserv.ipc.org/archives Please visit IPC web site
>> http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>> for additional information, or contact Keach Sasamori at
>> [log in to unmask] or 847-615-7100 ext.2815
>> -----------------------------------------------------
>> R
>>
>>
>> --
>> No virus found in this incoming message.
>> Checked by AVG Anti-Virus.
>> Version: 7.0.344 / Virus Database: 267.14.17/228 - Release Date:
>> 1/12/2006
>>
>>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
> unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
> or
> (re-start) delivery of Technet send e-mail to [log in to unmask]: SET
> Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
> posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
> archives of previous posts at: http://listserv.ipc.org/archives Please
> visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for
> additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
> unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
> or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET
> Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
> posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/
> archives Please visit IPC web site http://www.ipc.org/contentpage.asp?
> Pageid=4.3.16 for additional information, or contact Keach Sasamori at
> [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|