Subject: Re: [TN] (URGENT) Acrylic coating, conclusion.
Salt, from a cleaning system?
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Ingemar Hernefjord
Sent: Monday, December 05, 2005 4:24 AM
To: [log in to unmask]
Subject: [TN] (URGENT) Acrylic coating, conclusion.
Remember the production stop and the unique veils and crystal on the
boards?
This came to me from the guy who was invited to help us solve the
problem.
(a 'casette' is a PWB mounted on a metal cooler with channels for forced
air circulation)
> The lacquer problem is solved. I believe that the crystal on lacquer
> surface is salt from our cleaning system. The cleaning agent Vigon in
> the system normally has a solid content 0.5%. The BFB cassette, after
> machine cleaning, still remained a pretty amount of Vigon on inside.
> It is also very common that the cassettes are often
not
> completely dried before being lacquered. The salt within Vigon left
> inside cassette is believed to have diffused to the surface of lacquer
> following the water/moisture migrations. When water moleculars
>evaporated, the salt left on the surface form crystals. This
>assumption can also explain why the crystal patterns are always
>initiated at short edges of the cassette, where the moisture content
>is normally slightly higher because the water absorption is more
>pronounced along the edge of boards. Recommended not to use Vigon.
>
> With best regards
>
> Qiao Wang PhD
So, as many of you suspected, the higly alcaline Vigon200 was the root
case, or rather the cleaning machine maintenance. Thank you all for good
advice.
Ingemar Hernefjord
Ericsson Microwave Systems
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|