TECHNET Archives

November 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Wed, 2 Nov 2005 10:48:23 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Bev Christian <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="us-ascii"
From:
Bev Christian <[log in to unmask]>
Parts/Attachments:
text/plain (160 lines)
Bill,
Stannic is +4, not +3.
Bev
RIM

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of [log in to unmask]
Sent: November 2, 2005 10:44 AM
To: [log in to unmask]
Subject: Re: [TN] Lead-Free testing

Wrote this up for IPC, posted it in the past. Method provided below in
case  
you missed it.
 
 
Number: 
Date: 
Revision: 
Subject: Surface Lead Contaminant Detection Spot  Test 
1.0 Scope 
1.1 This  simple and rapid non-destructive colorimetric spot test method
is 
for use in  determining if non-ionic lead (primarily lead oxide)
contaminant is 
present on  bare printed wiring board and completed assembly surfaces.

1.2 The  test will not identify the particular compound of lead present
on 
the surface  tested nor separate mixtures of various lead compounds on
the 
surface.  After a functional problem is found with  boards or
assemblies, usually 
failure at elevated temperature and humidity, this  test can be used to
confirm 
or eliminate non-ionic lead contaminant as a root  cause. 
1.3 The test  can detect lead levels easily in the 0.1 microgram range.

Lower levels in the presence of  interferring metals can be detected by
a skilled 
operator using accurate  standards. 
2.0  Applicable Documents 
IPC-TP-135   "Insulation  Resistance Degradation by Non-Ionic Surface 
Contamination-- Its Cause &  Cure." 
Feigl , Fritz, and Suter, Hans A., "Analytical  Use of Sodium
Rhodiazonate", 
  Industrial  and Engineering Chemistry, Vol. 14, No. 10, 840-2,
(1942). 
3.0 Test Specimen 
3.1 A bare  printed wiring board or completed assembly at least 50 mm x
50 mm 
x  thickness. 
4.0  Apparatus & Materials 
4.1 Sodium  rhodizonate 
4.2  Tartaric  acid 
4.3 Sodium  bicarbonate 
4.4 Cotton  tip swabs 
4.5  Indicator dropper bottle 
4.6 Balance  capable of weighing to 0.001 g. 

5.0  Procedure 
5.1  Preparation 
5.1.1 Prepare  the stock buffer solution by dissolving 15 grams of
tartaric 
acid and 19 grams  of sodium bicarbonate in one liter of distilled
water.   The 
pH of the resultant buffer  solution should be 2.79.  This  solution is 
stable, and can be stored for an extended time in the  laboratory. 
5.1.2 Prepare  the 0.2% sodium rhodizonate indicator solution by
dissolving 
0.01 g. of sodium  rhodizonate in 5 ml. of water.  Place the solution in
the 
indicator dropper bottle.  [Note: the useful life of the indicator
solution is 
approximately 8 hrs.] 
5.2  Test 
5.2.1 Using a  clean cotton swab, place 2 drops of buffer solution on
the 
cotton swab.   
5.2.2 Rub the  buffer soaked swab on a dielectric area (non-plated area)
of 
the printed wiring  board or assembly surface, being sure not to touch
the  
traces. 
5.2.3 Using a  second clean cotton swab, place 3 drops of the indicator
on 
the cotton swab.   
5.2.4 Rub the  indicator soaked swab in the area coated by the buffer
swab. 
5.3  Evaluation  
5.3.1 Any  color change from yellow to red on the indicator swab
indicates a 
positive test  for lead contaminant.   
5.4 Action 
5.4.1 The  boards or assemblies should also be tested for the presence
of 
organic non-ionic  contaminant using the test methods cited in 2.0. 
5.4.2 The  lead contaminated boards or assemblies can be recovered by 
applying and curing  the laquer described in 2.0, then washing it off
using a 
suitable cleaning  agent.  
5.4.3 The  organic non-ionic contaminated boards or assemblies can be 
recovered per methods  cited in 2.0 
6.0 Notes 
6.1 The  tartaric acid, sodium bicarbonate and sodium rhodizonate used
in  
this method can be obtained from standard chemical supply houses.
Reagent grade 
chemicals are  preferred. 
6.2 The  literature claims this test can be used to detect the presence
of 
stannous tin  (+2 oxidation state) by a color change to violet, however,
stannic 
tin (+3  oxidation state) gives no change. 
Originally Drafted by:            W. G. Kenyon            April, 1998

Revised:                                 W. G. Kenyon            March,
2005 


Bill  Kenyon
Global Centre Consulting
3336 Birmingham Drive
Fort Collins, CO  80526
Tel: 970.207.9586 Cell: 970.980.6373
email:  [log in to unmask]

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------




---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2