Ingemar: What is the process you use for plating on to Kovar? This should work for Inconel as well.
The main issue, after you have gotten the Inconel clean, which could be a challenge, is to get it to plate without getting immersion Copper first, which would adhere loosely. In the "old days", platers got around the immersion plating problem by using alkaline Copper plating baths, such as Cyanide, or Pyrophosphate.
Since you also face the issue of immersion Copper on Kovar, whatever works for Kovar, would work well on Inconel.
Rudy Sedlak
RD Chemical Company
Ingemar Hernefjord <[log in to unmask]> wrote:
Ted,
We used copper on this alloy in order to make it solderable.
I'm not very familiar with plating in detail, but as far as
I remember we used a nickel strike followed by sulphuric acid
sulphate copper bath. The plated copper was 50 micrometers
thick (yes, that thick!). Upon that a gold flash. The plating
company said it was a piece of cake.
We use copper plating even on aluminium and Kovar.
Inge
-----Ursprungligt meddelande-----
Från: TechNet [mailto:[log in to unmask]] För Ted Edwards
Skickat: den 30 november 2005 03:14
Till: [log in to unmask]
Ämne: [TN] Plating Copper on INCONEL
We are looking for how to plate copper on INCONEL (a Nickel Chromium
Iron alloy, the alloy we are considering is INCONEL 600). Anybody have
any suggestions?
Ted Edwards
[log in to unmask]
(480)736-3728
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
Yahoo! Music Unlimited - Access over 1 million songs. Try it free.
|
|
|