TECHNET Archives

November 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, John Burke <[log in to unmask]>
Date:
Tue, 29 Nov 2005 12:52:44 -0500
Reply-To:
Subject:
From:
Joyce Koo <[log in to unmask]>
Content-Transfer-Encoding:
7bit
In-Reply-To:
Content-Type:
text/plain; charset="us-ascii"
MIME-Version:
1.0
Parts/Attachments:
text/plain (236 lines)
or the phone in your back pocket went into the washing machine?
                             jk

-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of John Burke
Sent: Tuesday, November 29, 2005 12:38 PM
To: [log in to unmask]
Subject: Re: [TN] Humidity and enclosed RF board


You mean apart from the one where my daughter ran into the ocean with a
mobile phone in her pocket??........................8-)

John

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Eric CHRISTISON
Sent: Tuesday, November 29, 2005 9:34 AM
To: [log in to unmask]
Subject: Re: [TN] Humidity and enclosed RF board

Agree with Richard about the environment. Letting the enclosure breathe
is
also a good plan; how many mobile phones fail due to humidity related
failures?

You might also consider adding a breathing desiccator to the enclosure
although they tend to be expensive and need replaced every six moths or
so.

Regards,



Eric  Christison
Mechanical Engineer
Home, Personal, Communication Sector - Imaging Division
STMicroelectronics
33 Pinkhill
Edinburgh
EH12 7BF

Tel:     +44 (0)131 336 6165
Fax:    +44 (0)131 336 6001



> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard
> Sent: Tuesday, November 29, 2005 5:25 PM
> To: [log in to unmask]
> Subject: Re: [TN] Humidity and enclosed RF board
>
>
> It also depends on the environment where the box will live.
> If it is near the sea, there is a much higher probability of
> failure if any moisture does enter from outside.
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Douglas O. Pauls
> Sent: Tuesday, November 29, 2005 11:01 AM
> To: [log in to unmask]
> Subject: Re: [TN] Humidity and enclosed RF board
>
> Well, it depends.
>
> You say that the casing seals the electronics from the
> external atmosphere. How well?  Is it a hermetic seal?  Are
> you using an elastomeric gasket? Do you package with an inert
> cover gas?  What is the design life of the product and what
> are the consequences of failure?
>
> In my experience, even those enclosures assumed to be
> "hermetic" are not, and that usually means moisture will
> eventually get in and will have a hard time getting back out.
>  So it all depends on how well insulated your case keeps the
> electronics throughout the design life. Elastomeric gaskets
> willl wear out.  Field repair is often less than optimal.
>
> If moisture gets inside the case, it will condense on your
> boards when you go through dew point.  Can it grow dendrites?
>  Yes.  What is the risk?  It Depends.  Dendrites have been
> observed to grow in as little as 3.5 volts DC.  There is no
> "safe" level of humidity because the degree of risk is
> dependent on both humidity and the amount of ionic soil.  The
> dirtier it is, the less humidity it takes.  Some papers have
> suggested 70% RH as a threshold, but this is usually SIR type
> of testing, not field trials.  In addition, if your product
> is functioning in some of the more polluted areas of the
> world, and the enclosure is not hermetic, then the pollutant
> gasses also get into the enclosure and do nasty things.
>
> Doug Pauls
>
>
>
>
>              "Tempea, Ioan"
>              <itempea@POSITRON
>              .QC.CA>
> To
>              Sent by: TechNet          [log in to unmask]
>              <[log in to unmask]>
> cc
>
>
> Subject
>              11/29/2005 10:43          [TN] Humidity and enclosed RF
> board
>              AM
>
>
>              Please respond to
>               TechNet E-Mail
>                    Forum
>              <[log in to unmask]>
>              ; Please respond
>                     to
>               "Tempea, Ioan"
>              <itempea@POSITRON
>                   .QC.CA>
>
>
>
>
>
>
> Hi Technos,
>
> application: one RF board and one antenna, no conformal
> coating, both sealed inside of a casing; outdoor unit, will
> see temp and humidity variations.
>
> question: assuming that the boards are well insulated from
> the exterior, should I worry about long term rel of the
> boards? Otherwise said, due to temp variations, can the
> residual humidity inside the casing condensate on the boards
> and cause damage? Or can it make grow dendrites?
>
> And a general question:  For dendrites we need a potential
> difference, humidity and dirt; is there any threshold for the
> humidity level, below which dendrites will not grow?
>
> Thank you,
> Ioan
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV
> 1.8e To unsubscribe, send a message to [log in to unmask] with
> following text in the BODY (NOT the subject field): SIGNOFF
> Technet To temporarily halt or
> (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE
> mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at:
> http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit
IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2