Hi Ingemar,
We have been aware for some time that the lead-content is higher near the IMC
layers, because some of the Sn has been used to form the IMCs. However, any
Pb-nonuniformity that might otherwise be present in solder joints would have
its impact felt [but not directly recognized] in the results of any accelerated
testing.
Now if there is a difference between the Pb-uniformity between the short-term
ACT samples and the long-term product solder joints, that is a different
matter--and I do not know how to currently address it.
We do, however, know of a difference between the short-term ACT samples and
the long-term product solder joints. that is the coarseness of the solder grain
structure which changes over time with temperature and loads. The difference
can be as high as a factor of 2 to 3. that is why IPC-SM 785 and IPC-9701
recommend artificially aging [meaning grain coarsening] solder joints prior to
ACT.
Werner
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|