TECHNET Archives

November 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Fri, 11 Nov 2005 09:13:17 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Kane, Joseph E (US SSA)" <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="us-ascii"
From:
"Kane, Joseph E (US SSA)" <[log in to unmask]>
Parts/Attachments:
text/plain (143 lines)
Dave:

According to TI, they used nickel/palladium until 2001,
then switched over to nickel/palladium/gold to save money.
Price of palladium had risen substantially, and NiPdAu
allowed them to plate thinner palladium.

Here's a link:
 
http://www.elecdesign.com/rohs/articles/Selecting%20the%20right%20RoHS%2
0finish.pdf

Palladium is a noble metal, so it shouldn't oxidize much,
but then again I've seen something that suggests that the gold
promotes faster wetting and better spread.  Can't find the reference.

-Joe

-----Original Message-----
From: David D. Hillman [mailto:[log in to unmask]] 
Sent: Friday, November 11, 2005 8:36 AM
To: [log in to unmask]
Subject: Re: [TN] Gold plated components, what a pain!!


HI Ivan! The purpose of the gold is to "protect" the Pd surface from
reacting with the environment. Pd is a "getter" material and can form a
number of "really neat" surface films, both oxide and/or organic films,
depending on the environment.

Dave Hillman
Rockwell Collins
[log in to unmask]




             Ivanoe Pedruzzi
             <i.pedruzzi@LABEL
             GROUP.COM>
To
             Sent by: TechNet          [log in to unmask]
             <[log in to unmask]>
cc

 
Subject
             11/11/2005 04:36          Re: [TN] Gold plated components,
             AM                        what a pain!!


             Please respond to
              TechNet E-Mail
                   Forum
             <[log in to unmask]>
             ; Please respond
                    to
              Ivanoe Pedruzzi
             <i.pedruzzi@LABEL
                GROUP.COM>






But Werner,

the 150 A is over Pd, does the Pd have different properties in terms of
oxidization, hence, soldering?

just for my understanding.

THX,
Ivan


Il giorno 10/nov/05, alle ore 23:16, Werner Engelmaier ha scritto:

> I agree that 150 Angstroms of Au "is pretty darn thin"--the problem is

> I see most layer thicknesses in the 500 to 1,000 A range. A 150A layer

> of au would
> not protect the Ni from oxidizing.
>
>
>
> Werner
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e To 
> unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail
> to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/
> archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?
> Pageid=4.3.16 for additional information, or contact Keach Sasamori
> at [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2