[log in to unmask] a écrit :
> Hi Arnaud,
> You do not give much of a description of your flex circuit. Thickness?
> Layer count? History? Bookbinder folds? Are you sure you have RA
> copper? It may be rolled, but not annealed and thus have high
> ductility in one direction and not the other. One way to determine
> that is to do an X-section--long needle-like grains are an indication
> opf insufficient annealing. Are there any unassembled circuits left?
> You could used IPC TM 2.4.3.2 “Flexural Fatigue and Ductility,
> Flexible Metal-Clad Dielectrics.”
>
> Regards,
> Werner Engelmaier
> Engelmaier Associates, L.C.
> Electronic Packaging, Interconnection and Reliability Consulting
> 7 Jasmine Run
> Ormond Beach, FL 32174 USA
> Phone: 386-437-8747, Fax: 386-437-8737, Cell: 386-316-5904
> E-mail: [log in to unmask], Website: www.engelmaier.com
>
Werner,
I already detailed the flex buid-up, but it's true it was a long time
ago: it consists of a 50µm polyimide core with two 35µm RA copper layers
covered by an adhesive of 50µm and a coverlay of 25µm.
A cross section of the copper traces followed by a chemical etching
showed a granular copper structure characteristic of a RA copper.
The design has already been pointed out and will be considered, but I
would like to ensure there is no manufacturing problem. I do not have
unassembled circuits, so my intention is to perform some comparative
hardness measurements on cross sectioned assembled boards as it was
discussed.
Arnaud
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|