Dear Gerard
This is interesting. I wonder what was the reason for incorporating Nickel
under layer then. Did it automatically derive from the spec for gold tabs ?
The reason for nickel in gold tabs was lower contact resistance. The direct
Gold shows what little copper oxide migrates on top is easily fluxed during
soldering.
Please correct me if I am wrong.
Anil Kher
micro interconnexion pvt. ltd
D3-12A, Corlim Industrial Estate
Corlim, Ilhas , Goa , India 403110
tel: 91-832-2284209/337. fax 2284209/2285271
e mail: [log in to unmask]
Leaders in Gold plated PCBs - selective/ cob
an ISO 9001-2000 Company
-----Original Message-----
From: Gerard O'Brien [mailto:[log in to unmask]]
Sent: Thursday, October 13, 2005 5:26 PM
Subject: Re: Direct Immersion Gold
Ryan - it has to do with density of the deposit. If you perform a porosity
test on DIG, the results mimic that of 30 microinches of gold rather than
the 2-4 microinches that is actually there. I have been testing in real time
DIG and using a wetting balance have a data set over 900 days of storage -
non protected office environment. If I compare my ENIG longterm test to DIG,
the DIG solders better at 899 days, wets faster and produces a higher
wetting force. The underlying Cu (oxide) I guess is easier to solder to than
a partially passivated nickel layer.
After 900 days it does not look very nice - rather brown in color but boy
does it solder.
Regards
Gerard O'Brien
Photocircuits.
-----Original Message-----
From: Ryan Grant [mailto:[log in to unmask]]
Sent: Wednesday, October 12, 2005 10:34 AM
To: [log in to unmask]
Subject: [TN] Direct Immersion Gold
Hi Techies,
Can anyone explain what direct immersion gold is?
My supplier gave me samples of several different board finishes, of which
two groups were direct immersion gold from two different suppliers. The
gold over copper was 5uin and 7uin, which I was surprised the copper hadn't
already diffused into the gold. I told him I had no interest in direct
immersion gold...but, since he gave me the samples, I might as well test
them with the samples that I am interested in (immersion silver). First, I
baked the boards at 125C for 48 hours to kill the solderability. Then they
were reflowed twice to kill solderability, and checked for wetting. Again,
I expected the copper to completely diffuse through the gold, and/or the
solderability to be dead. To my surprise, the gold was still there and
solderability was still good; whereas immersion tin and OSP showed evidence
of dewetting.
(ENIG and immersion silver still had good wetting too).
So can anyone explain why the copper and gold didn't diffuse into each
other?
Thanks,
Ryan
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per
day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|